Two hours at 210 °C (410 °F) take 43 MPa (6.2 ksi) off the horizontal yield strength of AlSi10Mg printed on an AddUp FormUp 350, from 275 to 232 MPa. On a Gränges powder sheet, two hours at 300 °C (572 °F) take the tensile strength from 447 to 285 MPa and lift elongation at break from 5 to 12 %. The alloy is the same, the powder is gas atomized to the same chemistry, and the heat treatment written on the purchase order decides which of those parts arrives.
AlSi10Mg is the aluminum casting alloy most often run in laser powder bed fusion (LPBF), where a laser melts thin layers of powder one over the other. Its printed properties behave unlike its cast properties, and the reasons sit in a microstructure that only exists because each melt pool freezes at cooling rates no casting reaches. The sections below read the makers’ datasheets, compare them with two published studies, and end with the lines a buyer writes into an order.
AlSi10Mg Tensile and Yield Strength by Heat Treatment
The first answer a buyer needs is the strength in each state the material is delivered in. Two makers publish it for their own systems and parameters, and their numbers are close enough to read together and different enough to show why the state and the source both travel with a figure.
| Source and state | Tensile strength | Yield strength Rp0.2 | Elongation at break | Young’s modulus |
|---|---|---|---|---|
| AddUp, as built, XY | 412 ± 38 MPa (59.8 ksi) | 275 ± 8 MPa (39.9 ksi) | 5 ± 2 % | 72 ± 3 GPa (10.4 Msi) |
| AddUp, as built, Z | 425 ± 30 MPa (61.6 ksi) | 239 ± 3 MPa (34.7 ksi) | 5 ± 2 % | 71 ± 5 GPa (10.3 Msi) |
| AddUp, stress relieved 210 °C (410 °F), 2 h, XY | 363 ± 7 MPa (52.6 ksi) | 232 ± 2 MPa (33.6 ksi) | 7 ± 2 % | 77 ± 4 GPa (11.2 Msi) |
| AddUp, stress relieved 210 °C (410 °F), 2 h, Z | 396 ± 20 MPa (57.4 ksi) | 230 ± 6 MPa (33.4 ksi) | 4 ± 1 % | 79 ± 7 GPa (11.5 Msi) |
| Gränges, as manufactured, Z | 447 MPa (64.8 ksi) | 241 MPa (35.0 ksi) | 5 % | 85 GPa (12.3 Msi) |
| Gränges, stress relieved 300 °C (572 °F), 2 h, Z | 285 MPa (41.3 ksi) | 184 MPa (26.7 ksi) | 12 % | 80 GPa (11.6 Msi) |
Sources: AddUp, AlSi10Mg Material Data Sheet, FormUp 350, 50 µm layers, ASTM E8, at least 27 specimens across the plate; Gränges, AM Material Datasheet AlSi10Mg, 50 µm layers, DIN EN ISO 6892-1 Method B, turned specimens.
The two stress relief temperatures explain most of the difference between the sheets. AddUp’s cycle at 210 °C keeps most of the as-built strength and buys two points of elongation in XY. Gränges’ cycle at 300 °C gives up roughly a third of the tensile strength and more than doubles the elongation. Neither is wrong; they are two different products, and “stress relieved” without a temperature describes neither.
AddUp also lists physical data next to the tensile rows: a typical relative density of 99.5 %, a theoretical density of 2.67 g/cm³ (0.0965 lb/in³), a thermal conductivity of 120 to 160 W/m·K at 25 °C, a melting range of 550 to 600 °C (1,022 to 1,112 °F) and a thermal expansion of 21 µm/m·°C (11.7 µin/in·°F) from 20 to 100 °C. Its footnote marks the thermal and electrical values as literature data, not measurements on printed parts. Gränges gives a printed part density of 2.68 g/cm³ (0.0968 lb/in³).
A strength figure for printed AlSi10Mg is incomplete without three things beside it: the heat treatment temperature and time, the build direction of the specimen, and the system it was printed on.
Chemistry Limits From EN AC-43000 and ASTM F3318
Both makers tie their powder to a published composition. Gränges quotes DIN EN 1706, the European standard for aluminum castings, under the designation EN AC-43000. AddUp states that its alloy complies with ASTM F3318, the ASTM specification for powder bed fusion of this alloy, and with EN AC-43000.
| Element | AddUp, ASTM F3318 and EN AC-43000 | Gränges, DIN EN 1706, EN AC-43000 |
|---|---|---|
| Silicon | 9.0 to 11.0 | 9.0 to 11.0 |
| Magnesium | 0.20 to 0.45 | 0.25 to 0.45 |
| Iron | ≤ 0.55 | ≤ 0.55 |
| Manganese | ≤ 0.40 | ≤ 0.45 |
| Titanium | ≤ 0.15 | ≤ 0.15 |
| Zinc | ≤ 0.10 | ≤ 0.10 |
| Copper | ≤ 0.03 | ≤ 0.05 |
| Nickel | ≤ 0.05 with tin and lead | ≤ 0.05 |
| Aluminum | Balance | Balance |
Sources: AddUp, AlSi10Mg Material Data Sheet, chemical composition table; Gränges, AM Material Datasheet AlSi10Mg, chemical composition table.
The two columns differ in the magnesium floor, the manganese ceiling and copper. Magnesium is the element that forms the Mg2Si precipitates a heat treatment works on, so a lot near 0.20 % and a lot near 0.45 % will not answer an aging cycle the same way. A buyer who needs the response of one lot to match the next names the specification on the order and asks for the powder certificate with each lot.
Powder Size and Packing
Gränges publishes its particle size distribution as D10 of 26 to 32 µm, D50 of 40 to 45 µm and D90 of 53 to 61 µm, measured on a Camsizer XT, with a tap density of 1.6 g/cm³ under ISO 3953 and an apparent density of 1.3 g/cm³ under ISO 3923-2. AddUp runs 20 to 63 µm spherical powder at 50 µm (0.002 in) layers. A study on the 3D Systems ProX DMP 320 used LaserForm AlSi10Mg0.3 powder of 10 to 63 µm. These ranges matter because the powder has to spread into a layer not much thicker than its largest particles, and a different cut of the same alloy is a different feedstock for the machine.
Why Printed AlSi10Mg Is Stronger Than Cast AlSi10Mg
A study in Scientific Reports printed AlSi10Mg on a 3D Systems machine and compared it with the same alloy cast and given a full T6 treatment. As built, the printed alloy reached a yield strength of 250 MPa (36.3 ksi) and an ultimate strength up to 435 MPa (63.1 ksi). The cast T6 reference reached 180 MPa (26.1 ksi) yield and 225 MPa (32.6 ksi) ultimate. Every printed condition in the study beat the cast reference.
The reason is scale. Inside each melt pool, measured at 189 ± 15 µm wide and 114 ± 8 µm deep, the aluminum freezes as cells averaging 0.46 ± 0.09 µm at the center of the pool and 0.89 ± 0.24 µm at its boundary, each wrapped in a network of silicon-rich eutectic. The authors estimated cooling rates on the order of a million kelvin per second at the pool center. At that speed silicon is trapped inside the aluminum cells: they measured about 2.7 wt% silicon in the cells, against a maximum equilibrium solubility of 1.65 wt% at the eutectic temperature.
Those two features, the fine cells and the trapped silicon, carry the strength. The layer below is reheated by the layer above, and the study shows a heat-affected band where the silicon network has partly broken up and rounded, which is one reason a printed part is not uniform on the scale of a melt pool.
What a Cast Heat Treatment Does to the Printed Structure
A T6 cycle starts with a solution anneal near 540 °C (1,004 °F), in the study 8 hours followed by a water quench, then ages at 160 °C (320 °F) for 6 hours. The anneal dissolves and coarsens exactly the structure that makes printed AlSi10Mg strong. Its authors conclude that applying T6 to printed AlSi10Mg removes the grain refinement and the silicon supersaturation, and with them the strengthening potential of the printed microstructure, and they reserve T6 for parts where that loss does not matter. For a part without internal channels or lattices, the same shape is usually cheaper as machined aluminum from 6061 or 7075 bar, so a printed AlSi10Mg part earns its place where the geometry cannot be reached by a tool.
Heat treatments written for castings were written for a coarse structure. On printed AlSi10Mg the same cycle starts from a far finer structure and ends wherever the anneal takes it.
Direct Aging, Stress Relief and Baseplate Heating Compared
The same study ran four printed conditions side by side, five machined round coupons per condition to ASTM E8M, built both horizontal and vertical. Its results give the clearest published picture of what each thermal choice trades.
| Condition | Thermal cycle | Yield strength | Ultimate strength | Thermal conductivity |
|---|---|---|---|---|
| As built | None | 250 MPa (36.3 ksi) | up to 435 MPa (63.1 ksi) | 124 ± 2 W/m·K (71.7 BTU/h·ft·°F) |
| Direct aged | 170 °C (338 °F), 6 h, furnace cool | 295 MPa (42.8 ksi) | 440 MPa (63.8 ksi) | 153 ± 5 W/m·K (88.4 BTU/h·ft·°F) |
| Stress relieved | 270 °C (518 °F), 2 h, furnace cool | 210 MPa (30.5 ksi) | 335 MPa (48.6 ksi) | 168 ± 4 W/m·K (97.1 BTU/h·ft·°F) |
| Plate preheated | Baseplate at 200 °C (392 °F) during the build | 160 MPa (23.2 ksi) | 310 MPa (45.0 ksi) | 183 ± 3 W/m·K (105.8 BTU/h·ft·°F) |
| Cast and T6, reference | 540 °C (1,004 °F) 8 h, water quench, 160 °C (320 °F) 6 h | 180 MPa (26.1 ksi) | 225 MPa (32.6 ksi) | Not reported |
Source: Van Cauwenbergh and co-authors, Scientific Reports, 2021, Table 1 for cycles, tensile results text and Table 2 for conductivity. Thermal conductivity was derived from measured electrical conductivity with the Wiedemann-Franz law.
Three readings follow from the table.
- Direct aging at 170 °C raises yield strength by 45 MPa over as built and keeps the ultimate strength, because silicon comes out of the supersaturated cells as fine precipitates while the eutectic network stays intact.
- Stress relief at 270 °C breaks the network into rounded silicon particles. Strength falls and conductivity rises, which suits heat sinks and housings where heat flow outranks strength.
- A hot baseplate during the build lowers the effective cooling rate. It gives the highest conductivity and the lowest strength of the printed set, and it is a machine setting rather than a furnace step, so it belongs in the order alongside the heat treatment.
The elastic modulus moves too. Measured by resonant ultrasound in the same study, Young’s modulus rose from 67.7 GPa (9.8 Msi) as built to 70.2 GPa after direct aging and 71.1 GPa (10.3 Msi) after stress relief.
A Second Study at 300 °C
A study in Discover Mechanical Engineering built 106 specimens on a central composite design and gave half of them a 200 °C baseplate and a stress relief at 300 °C (572 °F). The heat-treated group came out on average 16 HV1 softer than the untreated group across all parameter sets. Its highest tensile strengths were 484 MPa (70.2 ksi) untreated and 321 MPa (46.6 ksi) treated; the highest elongations were 8 % untreated and 16.3 % treated. Its hardness values in both states stayed above the minimum that DIN EN 1706 sets for cast AlSi10Mg in T6, which the paper gives as 75 HB or 79 HV1.
Build Direction and Elongation Along Z
Strength in AlSi10Mg changes modestly with direction. Elongation changes more. The Scientific Reports study found the vertically built coupons notably less ductile than the horizontal ones in the as-built, direct-aged and stress-relieved conditions. In the Discover study, specimens tested at 0°, 45° and 90° to the plate showed the 0° specimens the most ductile and the 90° specimens the least, and its statistics marked build orientation as a significant factor for elongation at break.
The AddUp sheet shows the same tendency after its 210 °C cycle: 7 ± 2 % elongation in XY against 4 ± 1 % in Z. As built, both directions read 5 ± 2 %.
A loaded feature that stretches across the layers, such as a bracket arm standing vertical on the plate or a thin boss built upright, is the feature that sees the lower number. Any design that needs elongation in one direction is best oriented on the plate so that direction lies in the layer plane, and a drawing that marks build direction lets the supplier hold that choice from lot to lot.
In printed AlSi10Mg, the direction that matters for ductility is the direction the layers stack, and the lowest elongation on a datasheet is usually the Z row.
Laser Parameters, Density and As-Built Roughness
Behind every datasheet row sits a parameter set: laser power, scan speed, hatch spacing and layer thickness. The Discover study varied them on 40 µm (0.0016 in) layers with a 67° rotation of the scan between layers, and found that laser power and scan speed carried most of the variation in density, roughness, hardness and strength. Its best density was 99.86 % at 300 W, 1,000 mm/s and a 0.14 mm hatch; its optimized set reached 99.96 ± 0.03 %.
A dataset in Data in Brief went further and printed 60 combinations on a 3D Systems ProX DMP 320 at 60 µm (0.0024 in) layers, from 60 to 460 W and 250 to 3,000 mm/s, with hatch spacing of 100 and 150 µm, deliberately reaching lack of fusion at one end and keyholing at the other. All of it was direct aged at 170 °C for 6 hours. The point for a buyer is the existence of those two failure regimes on either side of a dense window, and that a supplier’s parameter set is the thing that places a part inside it.
Surface Roughness in the As-Built State
The published roughness values for printed AlSi10Mg spread widely, and each belongs to its own surface and method.
- AddUp, vertical faces as built: Ra 6 to 8 µm (236 to 315 µin), optical profilometer, cutoff 2.5 mm.
- AddUp, vertical faces after bead blasting with glass medium at 2 bar (29 psi): Ra 4 to 7 µm (157 to 276 µin).
- Gränges, vertical faces as built: Ra 11 to 20 µm (433 to 787 µin) and Rz 70 to 170 µm (2,756 to 6,693 µin), to DIN ISO 13565-1 and -2.
- Discover study, top surface with its best parameter set of 350 W and 700 mm/s at 40 µm layers: Ra 2.0 ± 0.2 µm (79 µin).
The top surface in the study is the last melted layer, which is why it reads far smoother than any vertical wall on the datasheets. Both makers note that roughness depends on orientation and parameters, and Gränges states its values are an indication of what can be expected.
The study’s own discussion section adds a caution. Similar parameters on different machines have given inconsistent results in the literature, because laser sources, beam quality and calibration differ, and the authors call for better standardization and calibration of machines. A datasheet from one system is a starting point for another, never a transfer.
Ordering AlSi10Mg Parts With the Right State
The datasheets and studies above point to a short set of lines that make an order for printed AlSi10Mg unambiguous.
- Name the composition specification, ASTM F3318 or EN AC-43000, and ask for the powder certificate with each lot.
- State the heat treatment as temperature, time and cooling, never as a word. “Stress relieved at 210 °C for 2 h” and “stress relieved at 300 °C for 2 h” are different parts.
- Mark build direction on the drawing for any feature that carries load or needs elongation.
- Ask for witness specimens printed in the same build, machined and tested to ASTM E8 or ISO 6892-1, in the direction that matters.
- Write the surface finish per face, with the measuring standard and cutoff, and say whether bead blasting is acceptable.
- If the parts are heat sinks or housings, say so, since the cycle that maximizes conductivity is the one that gives up the most strength.
A part whose only requirement is “AlSi10Mg” can arrive in any row of Table 1 and still be correct. For a buyer deciding between low-volume 3D printing in AlSi10Mg and a cast or machined part for bridge production, the heat treatment line is the one that decides which of those parts the drawing is really asking for.
Sources and Further Reading
- AlSi10Mg Material Data Sheet, FormUp 350, version US-10252023-0129, AddUp
- AM Material Datasheet AlSi10Mg, revision 10.2023, Gränges Powder Metallurgy
- Unravelling the multi-scale structure–property relationship of laser powder bed fusion processed and heat-treated AlSi10Mg, Scientific Reports, 2021, Scientific Reports via PubMed Central
- Dataset of process-structure-property feature relationships for AlSi10Mg material fabricated using laser powder bed fusion additive manufacturing, Data in Brief, Data in Brief via PubMed Central
- Comprehensive study on statistical methods for optimization of process parameters and material properties of AlSi10Mg in laser powder bed fusion, Discover Mechanical Engineering, 2024, Springer Nature