A wall drawn 0.20 mm thick came out between 0.304 and 0.423 mm thick in an open-access study of 316L stainless steel, a size error of 52 to 111 % of the design. A gap drawn 0.20 mm wide between two such walls closed completely at high laser power. The test pieces were small, the machine was a research system and the walls were far thinner than most drawings carry, which is the reason the study is useful: it isolates what the laser does to a size, and shows that the dimension on a metal powder-bed part is partly a setting and not only a property of the machine.
This piece reads that study next to the published accuracy statements of EOS for its 316L process. It covers what the two sources claim, how the size error was measured, what laser power, contour scanning and orientation did to it, and how to write a requirement for walls, slots and gaps that a supplier can quote and a buyer can check.
Thin Wall and Gap Error in 316L Laser Powder Bed Fusion
The machine maker states accuracy as a band. EOS’s sheet for 316L, dated May 2014, gives a typical achievable part accuracy of about ±20 to 50 µm (±0.0008 to 0.002 in) for small parts and about 0.2 % for large parts, and a minimum wall thickness of about 0.3 to 0.4 mm (0.012 to 0.016 in). A footnote gives the basis: users’ experience of typical geometries, with about 40 µm when the parameters can be tuned for a class of parts and about 60 µm when a new kind of geometry is built for the first time, subject to data preparation and post-processing.
The current EOS sheet gives a different minimum wall for a different parameter set. The 40 µm layer set on the EOS M 290 lists 0.1 mm (0.004 in), and the 20 µm set lists 0.3 to 0.4 mm. Table 1 sets the statements together.
| Statement | Value | Basis |
|---|---|---|
| Typical part accuracy, small parts | about ±20 to 50 µm (±0.0008 to 0.002 in) | users’ experience on typical geometries |
| Typical part accuracy, large parts | about 0.2 % | same |
| Accuracy on a new geometry | about 60 µm (0.0024 in) | same, first build |
| Minimum wall, 20 µm parameter set | 0.3 to 0.4 mm (0.012 to 0.016 in) | EOS M 290, standard nozzle |
| Minimum wall, 40 µm parameter set | 0.1 mm (0.004 in) | EOS M 290, grid nozzle |
| Dimensional change after heat treatment | +0.02 % (20 µm set), +0.2 % (40 µm set) | typical, per parameter set |
Sources: EOS material data sheet for StainlessSteel 316L (current process data and the May 2014 edition).
A buyer reading the table has two numbers for the same thin feature, 0.1 mm and 0.3 to 0.4 mm, and no explanation on the sheet for why they differ. The study below does not explain EOS’s sets, since it ran on another machine, and it does show how a wall of designed thickness 0.2 mm grows into the 0.3 to 0.4 mm range when the laser is set to certain powers.
A minimum wall on a datasheet is a statement about a parameter set. The same wall drawn at another power or another contour setting prints at another thickness.
The Test Pieces and How Error Was Measured
A team at the University of South Carolina published the study in Engineering Science in Additive Manufacturing in 2025 under a Creative Commons license. Their specimens were groups of three walls, each nominally 0.20 mm thick, 3 mm high (a height to thickness ratio of 15 to 1) and 10 mm long, standing on a common base, with two gaps of equal nominal width between them at 0.2, 0.4 and 0.6 mm.
The conditions were as follows.
- Machine: an Aconity MIDI with a single-mode fiber laser of up to 1,000 W.
- Laser and layer: a 100 µm spot, a 100 µm hatch spacing and a 30 µm layer, at a fixed scan speed of 1,466.6 mm/s.
- Powder: gas-atomized 316L with a particle range of 15 to 45 µm and an average of 30 µm.
- Atmosphere: argon below 100 ppm oxygen.
- Conditions tested: laser powers of 260 W, 440 W and 620 W, each printed twice.
Dimensional error (DE) in the paper is the measured dimension minus the nominal one. The authors sectioned the specimens, photographed the polished cross-section, converted the image to black and white, and read the average wall thickness or gap at the half grey value across the section. Surface roughness (Ra) came from six outlines of the side wall per condition.
That method suits a study of mechanisms and differs from how a supplier inspects a delivered part. It measures a cut section at one height, in two specimens per condition, with a threshold chosen by the authors. The values are good for ranking the effect of settings and are not a capability statement for any production machine.
Laser Power Sets How Thick a Wall Prints
The walls grew with laser power. Table 2 gives the numbers the paper prints for its roughness and melt pool measurements and for the wall thickness.
| Laser power | Melt pool area | Wall thickness (nominal 200 µm) | Dimensional error | Vertical surface Ra |
|---|---|---|---|---|
| 260 W | 3,842 µm² | 304.3 µm (0.0120 in) | +104.3 µm (+0.0041 in) | 13.94 µm (0.00055 in) |
| 440 W | 6,399 µm² | not stated for this case | not stated | 19.32 µm (0.00076 in) |
| 620 W | 9,662 µm² | 422.9 µm (0.0167 in) | +222.9 µm (+0.0088 in) | 21.35 µm (0.00084 in) |
Source: Zhang and Yuan, Engineering Science in Additive Manufacturing, 2025. Melt pool area and Ra are for the 200 µm gap, contour scan group; the wall thicknesses are the figures the text gives between 260 W and 620 W.
Raising the power from 260 to 620 W enlarged the melt pool by 2.5 times (9,662 against 3,842 µm²), thickened the wall by 118.6 µm and raised the roughness by 7.4 µm. The authors explain it through melt pool behavior. A bigger pool spreads sideways into the powder next to the wall, and at the highest power it migrates toward the powder and forms dross, protrusions that stand outside the intended geometry.
For a buyer, the point is the direction. Every figure in Table 2 is oversize. A walled part printed on these parameters grows, and the size error has a sign.
A Contour Scan Cuts the Error by Roughly 40 to 45 Percent
The study tested two scan paths. In the first, only hatch scans were used, and they ran to the edge of the geometry. In the second, the hatch scan was offset inward by 50 µm and a contour scan ran along the boundary at the same power and speed.
The error ranges are clear. Without the contour, the wall dimensional error ran from 165.6 to 347.8 µm (0.0065 to 0.0137 in) across all conditions. With the contour and the inward offset it ran from 91.9 to 199.7 µm (0.0036 to 0.0079 in). The ratio of the two ranges is 1.80 at the low end and 1.74 at the high end, so the contour removed roughly 40 to 45 % of the error.
The authors’ reading is that the inner offset reduces the scanned area, compensating for the melt pool’s extent beyond the scan path, and that larger overlap with the inner hatches restricts migration and dross. They also warn that too large an offset risks lack of fusion between the contour and the hatch, which can compromise mechanical properties. A buyer cannot see any of that on a drawing, and the contour and offset are parameters the supplier holds in its parameter set. They matter for the same reason the process control heading exists in the purchasing standard: the dimension depends on a setting that has to be named.
Gaps Close Before They Widen
A gap is the mirror of a wall. Where a wall grows, the gap beside it shrinks. The study printed gaps of 0.2, 0.4 and 0.6 mm, and its results on them are the most practical for a designer of slots, channels and heat exchanger passages.
| Case | Nominal gap | Printed gap | Dimensional error |
|---|---|---|---|
| 620 W, 600 µm gap, no contour, perpendicular to gas flow | 600 µm (0.0236 in) | 216.7 µm (0.0085 in) | −383.3 µm (−0.0151 in), −64 % |
| High power (440 W and 620 W), 200 µm gap, no contour | 200 µm (0.0079 in) | closed | −200 µm (−0.0079 in), −100 % |
| All conditions, wall error without contour | not applicable | not applicable | wall +165.6 to +347.8 µm |
| All conditions, wall error with contour | not applicable | not applicable | wall +91.9 to +199.7 µm |
Source: Zhang and Yuan, 2025. The first two rows are the cases the paper states in numbers; the last two restate the wall error ranges for comparison.
The 600 µm gap lost 64 % of its width at 620 W with no contour scan, and the 200 µm gap vanished. The authors call the closed gap a functional failure of the part, and note that at small gaps the adjacent walls coalesce at high power, so the absolute error looks smaller (the gap is only 200 µm to lose) while the relative error reaches −100 %.
The paper gives a relation to estimate the final gap: Dg = DN − Doffset − Dw, where Dg is the final gap, DN the nominal gap, Doffset the contour offset (negative for an inward offset, or the distance of the outermost hatch line from the boundary if there is no contour) and Dw the melt pool width of the contour or outermost hatch track. When the inward offset equals the melt pool width, Dg equals DN and the error is minimal.
A worked case with assumed values shows the use. Take a nominal gap of 0.40 mm and a melt pool width of 0.12 mm, the second figure assumed here and not reported by the paper. With no offset the final gap is 0.40 − 0 − 0.12 = 0.28 mm, an error of −0.12 mm. With the study’s 50 µm inward offset the final gap is 0.40 + 0.05 − 0.12 = 0.33 mm, an error of −0.07 mm. A design that needs a 0.40 mm gap in service either draws 0.52 mm and prints near it, or asks the supplier to compensate its contour so that the gap lands on 0.40.
A narrow slot in printed metal is set by the laser offset as much as by the drawing. Draw the gap the part needs and let the supplier state how the parameters compensate for it.
Print Orientation Mattered Little in This Study
The authors printed the walls parallel and perpendicular to the gas flow and recoating direction. The differences in wall error between the two orientations ranged from −33.2 to +33.2 µm (±0.0013 in), with a maximal relative difference below 9.5 % of the overall error range. A three-way analysis of variance on the no-contour data found laser power significant (p below 0.0001) and gap distance significant (p = 0.0053) on the error, and orientation not significant (p = 0.5841).
For a buyer this is a narrow result. It says that rotating the walls in the plane of the plate did not change the error under these conditions, and nothing about tilting the part relative to the build plate or the effect of overhangs, which the study did not test. It also does not support dropping the build direction from a drawing, since the tensile data of the same alloy differ by build direction.
Roughness Sits Inside the Dimension
The vertical wall roughness in the study rose with power, from Ra 13.94 µm to 21.35 µm in thin walls and from 13.61 µm to 23.99 µm in 10 mm cubes. The EOS 2014 sheet states Ra 13 ± 5 µm for vertical surfaces as manufactured and Ra 5 ± 2 µm after shot peening. A roughness of Ra 13 µm is a dimension in its own right, a third of a 0.04 mm tolerance band, and the measured size of a surface depends on whether the gauge rides on the peaks or in the valleys. The paper notes that the top surface of thin walls can carry humps of about 200 µm at higher power, which belongs to the geometry and no gauge removes.
Writing a Thin Feature Requirement for Printed 316L
ISO/ASTM 52902:2023, published on 23 August 2023, describes benchmarking test pieces, called artefacts, and the measurements to take on them, so that the geometric performance of an additive system can be evaluated or calibrated. It gives a suite of test geometries aimed at specific performance metrics, specifies what to measure and the quality of the measurement, and does not prescribe the measurement method or how the pieces are built. A supplier that has run such artefacts holds capability data for the feature types in its own words.
The lines below use the study and the standard together.
- State minimum wall and minimum gap as a requirement on the part, with the parameter set the supplier uses to reach it, and ask for the printed result on a sectioned witness feature.
- Write the gap that the part needs in service, not only the gap on the file, and ask how the contour offset compensates for melt pool width.
- Write whether a size applies as built, after heat treatment or after finishing, because the dimensional change after heat treatment is listed per parameter set.
- Give the roughness and its measure with the dimension, as Ra or Sa, and the surfaces it applies to.
- Ask the supplier for capability data from test artefacts for the features used, and for the number of builds behind it.
- For any feature tighter than about ±0.05 mm, write a machining allowance and the tolerance on the machined surface.
For a buyer weighing low-volume 3D printing in metal against a machined or cast part for bridge production, the walls, slots and gaps are where the printed part differs most from the drawing, and they are the features to measure on the first article.
Sources and Further Reading
- Tianyu Zhang and Lang Yuan, Dimensional accuracy and surface roughness of thin-wall geometries in laser powder bed fusion of 316L stainless steel, Engineering Science in Additive Manufacturing, volume 1, issue 3, 2025, doi 10.36922/ESAM025340022 (open access, Creative Commons Attribution license). https://journal.hep.com.cn/esam/EN/PDF/10.36922/ESAM025340022
- EOS GmbH, Material data sheet EOS StainlessSteel 316L with process data for EOS M 290 and EOS M 400-4. https://www.eos.info/metal-solutions/metal-materials/data-sheets/mds-eos-stainlesssteel-316l-4441
- EOS GmbH, Material data sheet EOS StainlessSteel 316L, HHE/05.2014, typical achievable part accuracy, minimum wall and surface roughness. https://www.eos.info
- Genorma, ISO/ASTM 52902:2023 Additive manufacturing, Test artefacts, Geometric capability assessment of additive manufacturing systems, catalog page (scope). https://genorma.com/en/standards/iso-astm-52902-2023
- Genorma, ISO/ASTM 52901:2017 catalog page and contents (clause 4.3.3 Tolerances, 4.3.9 Process control information). https://genorma.com/en/standards/iso-astm-52901-2017