A test bar of Accura ClearVue printed on a 3D Systems ProJet 6000 HD measured an Ra of 1.733 µm (68 µin) on the face built flat, 2.686 µm (106 µin) on the face built at 30° and 1.649 µm (65 µin) on the vertical face. Its tensile strength barely moved with orientation. In a resin part, orientation rarely decides how strong the part is; it decides which faces carry support marks, which faces show steps, where trapped resin can spoil the print, and whether the part stays on the platform until the last layer.
Stereolithography (SLA) and its projection relatives cure liquid photopolymer layer by layer with ultraviolet light. Orientation and supports are set in software before anything is printed, and they are the step where most print failures and most cosmetic complaints are decided. The sections below walk that step in the order it is done, from naming the faces that matter through to the support pattern, with what goes wrong at each stage and how it shows on the part. Those working rules come from published design guides by Carbon and Stratasys for their vat photopolymerization printers and from studies of SLA parts; where a rule belongs to one maker’s process, the text says so.
The Orientation Step in Order
The order below follows Carbon’s published assessment criteria for orientation and supports, with Stratasys’s design guide filling in thresholds.
- Name the critical features: holes, fits, bonded faces, snap fits.
- Name the cosmetic faces that buyers will look at.
- Turn the part so overhangs and bridges use self-supporting angles where the critical and cosmetic faces allow it.
- Check how the cross section changes from slice to slice and how much of the part sits on the platform.
- Find and vent any volume that traps resin.
- Add supports where the part still needs them, choosing the type for each face.
- Compare print time, resin and labor across the options that remain, and against how many parts fit in one build.
Carbon recommends starting from its software’s automatic orientation and then assessing the result against these criteria; it also says plainly that more than one solution may print successfully, and that the choice balances priorities against the printer’s dynamics.
Checks Before the Part Is Turned
Stratasys’s guide opens with a short checklist that belongs before any orientation is tried, because each answer limits the orientations worth trying.
- Is a suitable material available for the application?
- Will the part fit inside the build volume in the preferred orientation? The bounding box of the part as oriented has to fit the envelope for the part to print in one piece.
- Are there features or walls smaller than 200 µm (0.008 in)?
- Are there overhangs, and will any critical surface need supports?
- Are there areas where resin cannot escape?
The same guide gives the fine-feature limits of its own printer, which set the floor for what orientation can rescue: an XY resolution of 50 µm (0.002 in), a minimum through hole of 0.2 mm (0.008 in), negative features of about 0.4 mm (0.016 in) and positive features down to about 0.2 mm, all dependent on material, orientation and geometry. A feature below those limits does not print in any orientation, and the part goes back to design rather than to the support software.
Cleaning and post-curing also enter here. Stratasys notes that viscous resins are harder to clean than low-viscosity rigid ones, so a part in an elastomer is oriented with drainage in mind from the start. The Arizona State study found its ProJet bars within two percent of their specified width and thickness, a reminder that an oriented and supported part is still measured after cleaning and cure, not on the screen.
Orientation is chosen for the faces that matter first. Every rule about angles and supports comes after the critical and cosmetic faces are named.
Self-Supporting Angles, Overhangs and Islands
The first test of any orientation is how much of the part needs support. Carbon lists the conditions: any feature that projects horizontally or below the self-supporting angle, any feature that starts printing before it connects to the rest of the part, too little contact with the platform at the start of the print, and any case where the part needs help to withstand the suction forces of printing.
| Condition | Carbon, DLS printers | Stratasys, Origin One |
|---|---|---|
| Self-supporting angle from horizontal | 40° or more most common, per resin | Steeper than about 30° usually self-supporting |
| Horizontal overhang needing support | Over about 2 mm (0.079 in) for most resins | Over about 3 mm (0.12 in); 1 to 2 mm usually safe |
| Bridge span needing support | Measured against the same 2 mm guide | Over about 10 mm (0.39 in) |
| Islands, features that start in mid-air | Always supported | Always supported |
| Elastomers | Thresholds set per resin | Shorter critical length and steeper critical angle than rigid resins |
| Drain hole for enclosed volumes | Venting through supports or reorientation | 3 mm (0.12 in) minimum |
| Unsupported wall | Per resin | 0.25 mm (0.010 in) minimum, 0.5 mm (0.020 in) recommended |
Sources: Carbon, Orientation and Supports; Stratasys, Origin One Design Guide. Both state that the values depend on the material.
The two makers do not agree on the angle, and they do not need to. Each publishes the threshold for its own resins and machines, and both say the figure depends on the material. Stratasys adds a failure to watch for: printing a face shallower than its 30° guide leaves layers that do not adhere, seen as peeling on the part.
Reorienting Before Adding Supports
Carbon’s examples show reorientation removing supports altogether: a part tilted so every downward face uses a self-supporting angle, and a tall part whose center of mass was far from the platform, reoriented so it needed no supports at all, gained a consistent cross section and printed faster. Stratasys gives the design-side alternatives: add fillets, chamfers or ribs to make geometry self-supporting, shorten or angle horizontal features, and remove features the part does not need.
Cross Section, Platform Contact and Suction
A vat printer pulls each new layer away from the window or the vat floor, and that separation pulls on the part. Stratasys describes these separation forces as occurring between layers whenever the build plate moves to let fresh resin flow in, and warns that a part not attached firmly enough to the build plate can be damaged or fall off. Carbon describes the same forces as suction and gives the orientation rules that follow from them.
- A large cross section on the platform holds well but is hard to remove, and rigid, brittle resins can chip on removal.
- A small cross section on the platform under a large cross section late in the print is the classic setup for an adhesion failure.
- An abrupt change in cross section, such as a bridge that suddenly closes, leaves a visible line on the part where the slice area jumps.
- Tall, top-heavy or asymmetric parts with a small footprint need stability supports, and the usual defect when they lack them is under-adhesion.
The remedy in each case is a reorientation that makes the cross section change gradually and keeps the height small relative to the footprint, or supports that add stability. Carbon’s guide says thin fence supports can buckle when tall, so stability supports use bar supports or thickened fence walls.
A part that fails late in the print usually failed in the software. Its cross section grew faster than its grip on the platform.
Trapped Resin and Venting
A cavity that is open only on the side facing into the resin holds liquid at low pressure while it prints. Carbon calls these unvented volumes and lists the defects they cause or worsen, including fringing, and notes a less obvious one: resin trapped in the part can leave too little liquid in the reservoir to finish the print. Its example is a part printed directly on the platform whose six holes trapped resin until the cassette ran short.
Carbon’s quiz on the subject makes the rule concrete. A cup printed open at the top is still unvented during printing, because the opening sits below the resin surface until the platform rises at the end. Lifting the part onto supports vents it through the gaps between them; reorienting can remove the trapped volume altogether.
Stratasys states the design rule from the other side: a fully enclosed volume cannot let resin escape and leaves uncured resin inside the finished part, so every enclosed volume needs a drain hole, 3 mm minimum on the Origin One. It also notes that viscous resins such as elastomers are harder to clean out than rigid resins, which matters for any cavity that has to drain after printing.
Choosing Supports and Where Their Marks Land
Supports are printed in the same material as the part and removed after printing, and each one leaves a mark. Carbon describes two kinds.
- Bar supports break farther from the surface and leave larger nubs. They are thicker and truss together, which makes them the choice for stability.
- Fence supports break close to the surface and leave smaller, evenly spaced nubs. They suit faces where marks matter but can buckle if tall.
The placement rules follow from the marks. Keep supports off critical features where an orientation allows it; where it does not, use fence supports to keep the nubs small. Put supports on faces that will be hidden, bonded or sanded. Carbon’s bracket example moved every support to the edges so the flat faces that had to sit tightly against other components stayed clean, and its name-plate example angled the plate so supports landed on the back rather than the front.
Supports also cost. Carbon notes that more supports mean more resin and more cost, and that orientation has a measurable effect on print time; it adds that the shortest print time often conflicts with the most parts per build, so both are weighed together.
Faces, Finish and Accuracy by Orientation
After supports, orientation decides how each face looks and how accurate each feature is.
Cosmetic Faces
Carbon’s guide names three visible effects of orientation on its printers: flow lines on large faces parallel to the platform, vertical lines on vertical faces from the corners of the image pixels, and visible slice edges on shallow curves. Each is reduced by tilting the cosmetic face out of that plane. Angled faces give the most consistent finish because the effects average out, and matching the angle of several faces gives them the same finish. Thinner slices reduce the slice edges on shallow curves at the cost of print time.
Measured Roughness by Angle
| Study, machine and resin | Flat | Angled | Vertical | Method |
|---|---|---|---|---|
| ProJet 6000 HD, Accura ClearVue | Ra 1.733 µm (68 µin) | Ra 2.686 µm at 30°, 2.546 µm at 60° (106 and 100 µin) | Ra 1.649 µm (65 µin) | Non-contact |
| SLA, XJRP-SPS600, 0.1 mm layers | Ra about 17 µm at 10° (669 µin) | Falls as angle rises | Ra about 3 µm at 90° (118 µin) | Contact |
| Masked SLA, 0.02 to 0.04 mm (0.0008 to 0.0016 in) layers | Lowest Sa at 0° | Angle the second factor after layer thickness, tested to 45° | Not tested | Optical, areal |
Sources: Golhin and co-authors, Surface roughness of as-printed polymers, Table 10; Arizona State University study in Materials; Black Sea Journal of Engineering and Science study on masked SLA.
The rows disagree on which angle is worst, and that disagreement is the finding. On the ProJet the flat and vertical faces are smoothest and the angled faces roughest; on the older XJRP machine roughness fell steadily as the angle rose. The masked SLA study found layer thickness mattered most, then angle, with exposure time a small factor, and post-curing lowered roughness by 8 to 11 % in every group. A study of a desktop SLA printer listed in the same review found that aligning models across the front of the platform, reducing overhangs, using supports and choosing a high resolution improved precision.
Critical Features
Carbon explains that some ultraviolet light passes through the edges of thin features, curing a little extra resin: overcure across the XY plane and cure-thru along Z. Because overcure acts evenly in XY, critical features hold better accuracy in that plane, while a vertical round feature comes out marginally oblong. Stratasys adds that overcure can partly fill a small hole, and that holes printed perpendicular to the build head come out most accurate. For parts that will be assembled, Carbon recommends orienting each part the same way relative to how they fit together.
Strength
The Arizona State study printed ASTM D638 tensile bars in three build orientations and several angles on the ProJet 6000 HD and found no statistically significant effect of orientation on modulus, strength or elongation, classing the parts as isotropic. It found a much larger effect from age: strength rose from 24 to 54 MPa (3,480 to 7,830 psi) for flat bars tested at one week and at six months. For SLA, the orientation step can usually be decided on faces and features, with strength checked after full cure rather than through orientation. Orientation matters twice when the print is a master for a silicone mold rather than a part, because every support mark and layer step on the master is copied into each casting.
What Goes Wrong and How It Shows
Each failure of the orientation step leaves its own sign on the part.
| What is seen | Likely cause in orientation or supports | Remedy named by the maker |
|---|---|---|
| Part missing or torn from the platform | Small footprint under a large late cross section; suction | Reorient for a consistent cross section; add supports |
| Under-adhesion on a tall part | Top-heavy or asymmetric part, small footprint | Stability supports, bar or thickened fence; lower height to footprint |
| Horizontal line across the part | Abrupt change in cross section | Reorient for gradual change |
| Shallow witness lines | Change in resin flow, platform entering and leaving the resin | Tilt the part to break surface tension gradually |
| Fringing or defects near a cavity | Unvented volume | Lift on supports or reorient to vent |
| Peeling layers on a sloped face | Face shallower than the self-supporting angle | Support it or steepen the angle |
| Chipped base | Large cross section on the platform in a brittle resin | Lift on supports; sand the nubs |
| Oblong vertical hole | Cure-thru along Z | Orient critical holes in XY |
Sources: Carbon, Orientation and Supports; Stratasys, Origin One Design Guide.
The buyer’s check on this step is simple to ask for. A screenshot of the oriented and supported part, showing which faces carry supports, settles most cosmetic disputes before a print starts, and a note of the build angle of critical features explains any oblong hole after it ends.
For a buyer weighing low-volume 3D printing of resin parts against molded parts for bridge production, marking on the drawing the faces where no support may touch is the one line that carries this whole step into the order.
Sources and Further Reading
- Orientation and Supports, Carbon
- Stratasys Origin One Design Guide, Stratasys
- Mechanical Anisotropy and Surface Roughness in Additively Manufactured Parts Fabricated by Stereolithography (SLA) Using Statistical Analysis, Materials, 2020, Arizona State University via PubMed Central
- Impact of Printing Parameters and Post-Curing on Surface Quality in mSLA 3D Printing, Black Sea Journal of Engineering and Science 9(2), 2026, Afyon Kocatepe University via DergiPark
- Surface roughness of as-printed polymers, a comprehensive review, International Journal of Advanced Manufacturing Technology 127, 2023, Springer Nature