HP’s design guidance for Multi Jet Fusion asks for a gap of 0.4 mm (0.016 in) between two printed parts that are made separately and then fitted together, split as 0.2 mm for each part. Parts printed already assembled, such as a hinge built in one piece, need at least 0.7 mm (0.028 in). A laser sintering guideline from the University of Zurich gives 0.2 mm for separately made moving parts and 0.5 mm (0.020 in) for parts made inside each other. Any clearance that is right for a pair fitted after printing is too small for the same pair built in place, because the gap in a powder bed has to empty of powder before anything can move.
None of these figures is a fit class in the sense of a machined shaft and hole. They are starting values from makers and labs, and HP says plainly that its references are not specifications and that a few iterations may be needed. The sections below set out the published values, explain the three reasons a printed fit closes up or opens out, walk a clearance stack for a pin and bore, and finish with how a fit is tested and written into an order.
Starting Clearances for Snug and Sliding Fits in SLS and MJF
A snug fit here means two printed parts that assemble with little play and stay together; a sliding fit means two parts that move against each other after assembly. The published values separate them by how the parts were made, more than by how tight the fit is meant to be.
| Case | Clearance | Process and source | Conditions printed with it |
|---|---|---|---|
| Parts printed separately, fitted together | 0.4 mm (0.016 in) gap, ±0.2 mm (±0.008 in) for each part | HP Multi Jet Fusion design guidance | Validated with HP 3D High Reusability PA 12, PA 12 GB and PA 11 |
| Parts printed as an assembly, moving | 0.7 mm (0.028 in) minimum between faces | HP Multi Jet Fusion design guidance | Walls 30 mm (1.18 in) thick or more need a larger gap |
| Parts printed as an assembly, thin walls | Down to 0.3 mm (0.012 in) | HP Multi Jet Fusion design guidance | Walls under 3 mm (0.12 in), subject to design and testing |
| Moving parts made separately | 0.2 mm (0.008 in) | University of Zurich, SLS design guideline | Laser sintered polyamide |
| Moving parts made inside each other | 0.5 mm (0.020 in) | University of Zurich, SLS design guideline | Laser sintered polyamide |
| Moving parts made separately and vibratory ground | 0.0 mm | University of Zurich, SLS design guideline | Clearance comes from the finishing |
Sources: HP, How to design a 3D print model, section on HP Multi Jet Fusion; University of Zurich, Design Guideline SLS, Connecting and Moving Parts.
The two sources agree in direction and differ in size. Both make the in-place figure larger than the separate figure, by 0.3 mm in each case. HP’s separate figure is twice Zurich’s, which reflects either a different process, a different reading of the number, or both: HP states its 0.4 mm as a gap split between two parts, and Zurich does not say whether its 0.2 mm is a gap per side or a difference in size.
For a snug fit between separately printed parts, the published figures give 0.2 to 0.4 mm as the place to start. Where a part will slide, the same starting gap applies when the parts are made apart, and the in-place figures apply when they are built together. Neither source gives an interference or press-fit value for a powder bed part.
A printed clearance is first a question of whether the parts are built apart or together. Built together, the gap has to release its powder before it can be a fit at all.
Printed Together or Assembled After Printing
A pair printed in place sits in the powder cake with loose powder filling every gap. The gap closes in two ways: heat from the walls on either side sinters some of the powder in it, and loose powder packed in the gap has to be blown or blasted out. HP’s guidance ties the gap to the wall thickness on each side for this reason: walls 30 mm thick or more need a larger gap, and walls thinner than 3 mm can work with as little as 0.3 mm. A thick wall holds more heat for longer.
The Zurich guideline adds the cleaning side of the same problem. It asks for escape holes of at least 4.0 mm (0.157 in), with at least two opposite each other, wherever powder has to leave a cavity, and sets the minimum hole diameter at 1.5 mm (0.059 in), with a note that it depends strongly on hole length and wall thickness. A sliding pin inside a closed sleeve, printed in place, needs a way for the powder in its gap to leave.
When Assembly After Printing Is the Better Choice
Printing apart costs an assembly step and gains a smaller clearance and a fit that can be checked before the parts meet. It also opens the finishing options the Zurich guideline lists: holes can be reamed if they are straight and accessible, and vibratory finishing can bring a separately made moving pair to zero designed clearance. Vibratory finishing reaches only external surfaces and suits parts without fragile pins or free thin walls.
Why Printed Holes Come Out Small
A drawing gives the pin and the bore their nominal sizes. Printed bores and printed pins do not land on those sizes in the same way, and the difference decides how much of the designed clearance survives.
| Process and source | Feature | Published behavior |
|---|---|---|
| SLS PA12, ProX SLS 6100, 50 parts | Inner diameters | Consistently undersized by about 0.1 mm (0.004 in) |
| SLS PA12, same study | Outer diameters | Close to nominal |
| SLS PA12, earlier study cited by the same paper | Inner and outer diameters | +0.1 / −0.6 mm inner, −0.1 / +0.6 mm outer (+0.004 / −0.024 in, −0.004 / +0.024 in) |
| SLS PA12, same study | Position near platform edge | Deviations increase by up to 0.1 mm (0.004 in) |
| Vat photopolymerization, Stratasys Origin One | Small holes | Overcure can partially fill the gap; minimum through hole 0.2 mm (0.008 in) |
| Vat photopolymerization, Carbon DLS | Vertical features | Cure-thru from below makes them marginally oblong |
Sources: International Journal of Advanced Manufacturing Technology study on SLS PA12 orientation and placement; Stratasys Origin One Design Guide; Carbon, Orientation and Supports.
The SLS study printed its parts on a 3D Systems ProX SLS 6100 with 100 µm (0.004 in) layers, a chamber at 167.5 °C (333.5 °F) and a 62 W laser, using the machine’s material scaling of 4.233 % in X, 4.423 % in Y and 2.4 % in Z, and measured them by X-ray computed tomography. Even with those scale factors applied, its bores came out about 0.1 mm small while outer diameters held nominal. The authors cite an earlier study with the same pattern at a wider range.
For a fit, that pattern is one-sided. A bore that prints small and a pin that prints true take clearance away; they never add it.
Overcure and Cure-Thru in Resin Parts
Vat photopolymerization moves holes the same way for a different reason. Carbon explains that resin is not completely opaque to ultraviolet light, so a little extra resin cures at the edges of features: overcure in the XY plane and cure-thru along Z. Overcure acts equally across the plane, so a critical feature keeps better accuracy oriented in XY; a vertical feature gets cure-thru only from below and comes out marginally oblong. Stratasys gives the same caution for its Origin One, where overcure can partially fill a small hole, and recommends printing a hole perpendicular to the build head for the most accurate and smallest holes. It states an XY resolution of 50 µm (0.002 in) for that machine and suggests 0.4 mm as a workable negative feature size.
Orienting Mating Features for the Fit
Orientation decides which of these errors a pair of mating features receives. The sources give four rules that apply directly to fits.
- Keep critical round features in the XY plane where the part allows it, since in resin processes overcure is even across that plane. Carbon gives this for its process.
- Keep supports off mating faces. Carbon’s example is a bracket whose flat faces needed a tight fit with other components, oriented so that supports land only on its edges; where a support cannot be avoided, fence supports leave smaller nubs than bar supports.
- Orient parts that will be assembled consistently relative to how they fit together, so every axis in each part sees the printing forces the same way. Carbon recommends this for assemblies.
- In a powder bed, weigh diameter against shape. The SLS study found horizontal orientations good for accurate inner diameters but worse for cylindricity, and one of the five orientations tested gave the highest cylindricity errors.
Carbon also lists the features that need this attention: holes for a press fit or for specific hardware, surfaces bonded to another component, and snap fits. A fit that matters gets its orientation chosen for the fit, and other choices follow.
Surface Texture on Sliding Faces
A sliding fit runs on its surfaces, and printed surfaces are rough at the scale of a clearance. One review of as-printed polymer roughness in the International Journal of Advanced Manufacturing Technology lists laser-sintered PA12 at an Ra of 13.4 µm (528 µin) and MJF PA12 at 11.9 µm (469 µin) in one comparison, and in another found MJF bottom faces at about 6.31 µm against 15.58 µm on top faces. Against that, a clearance of 0.2 mm is 200 µm; the peaks of two such faces take a measurable share of it, and they wear down in the first cycles of sliding.
The practical consequences follow from the sources.
- A sliding face benefits from being a down-facing surface in MJF, where the review records the smoother skin.
- A vibratory finish, as the Zurich guideline notes, can take a separately made moving pair to zero designed clearance, which means the finishing removes enough material to be part of the fit.
- A bore that will carry a sliding pin can be reamed after printing if it is straight and accessible, which turns the printed bore into a machined one.
A Worked Clearance Stack for a Printed Pin and Bore
The arithmetic below uses the published numbers with stated assumptions. It is a way to read the sources, not a measured result.
Assume a 10 mm (0.394 in) pin and its bore, printed separately in PA12 in a powder bed, designed with the HP starting gap of 0.4 mm on diameter: bore 10.4 mm, pin 10.0 mm.
- The bore prints about 0.1 mm small, per the ProX study: 10.3 mm.
- The pin prints close to nominal: 10.0 mm.
- The remaining clearance on diameter is 0.3 mm (0.012 in), or 0.15 mm per side if the pin is centered.
- If the bore sits near the edge of the platform and its position moves by up to 0.1 mm relative to another feature on the same part, a second pin in the same part loses up to that amount on one side.
- Surface peaks of the order of the Ra values above sit on both faces.
The pair still fits, with less play than drawn. Built in place instead, with the same 0.4 mm gap, the pair falls below HP’s 0.7 mm minimum for printed assemblies and risks a gap that never clears of powder.
The same stack in resin replaces step 1 with overcure, whose size the sources describe without a figure, and adds the support nubs of any support on a mating face.
Roundness Takes Its Share Too
Diameter is not the only error in the stack. The SLS study cites earlier work in which the roundness of cylindrical SLS PA12 parts varied between 0.15 and 0.5 mm (0.006 and 0.020 in), with higher laser power increasing the error and horizontal placement giving the best result, and another in which regular SLS PA12 specimens showed a maximum form deviation of 0.4 mm (0.016 in). A bore that is 0.3 mm larger than its pin on average but out of round by a similar amount will touch the pin on its short axis. For a fit that has to turn rather than only assemble, roundness belongs in the stack beside diameter.
The printed bore is the feature that moves. A clearance written for a machined pair loses part of itself to the bore before the parts ever meet.
Pins, Clips and Long Rails in a Printed Fit
The features that make up a fit have their own size limits, and the sources give them.
- Pins. The Zurich guideline gives 0.5 mm (0.020 in) as the minimum printable pin diameter and 1.8 mm (0.071 in) for reproducible results and good mechanical properties, notes that strength depends on length relative to diameter, and suggests hollow pins or internal support from 8 mm (0.31 in) upward.
- Walls of clips and sleeves. HP gives a minimum of 0.3 mm (0.012 in) for short walls in XY and 0.5 mm (0.020 in) for short walls in Z; Zurich asks for 1.0 mm (0.039 in) for reproducible results on supported walls in SLS.
- Cantilevers such as snap arms. HP ties the minimum thickness to the aspect ratio and asks for an aspect ratio below 1 for cantilevers under 1 mm wide.
- Long sliding rails. HP warns that parts with an aspect ratio above 10:1, abrupt changes of section or long thin curved segments are susceptible to warpage from uneven cooling, and suggests thicker walls, smoother transitions and hollowing or lattices to reduce it. A rail that bows by a fraction of a millimeter uses up a clearance of the same size along its length.
Testing and Specifying a Printed Fit
Every source ends in the same place: test the fit. HP says its values are estimates of a good starting design parameter, affected by the design of the part, and that iterations may be needed. The SLS study calls for validation across other machines and materials before its findings are generalized.
A fit coupon answers the question for one machine, material and orientation. Useful coupons carry the actual pin and bore pair at three or four clearances around the starting value, printed in the orientation and position the production parts will have, and assembled the way the parts will be assembled.
The order then carries the result:
- the clearance on diameter for each mating pair, stated as the assembled play that is acceptable;
- whether the parts are printed apart or as an assembly;
- the build orientation of each mating feature;
- whether bores may be reamed or faces finished, and whether the fit is checked before or after finishing;
- that supports may not touch mating faces, in resin processes;
- the gauge or method used to accept the fit, such as a go and no-go pin.
For a buyer weighing low-volume 3D printing of an assembly against molded parts for bridge production, the fit coupon is the cheapest step in the program, since it turns a published starting gap into a measured one before a full batch is built.
Sources and Further Reading
- How to design a 3D print model, HP Multi Jet Fusion design tips, HP
- Design Guideline SLS, University of Zurich, Additive Manufacturing Facility
- Influence of part orientation and spatial placement on the dimensional and surface quality of SLS-printed PA12 components, International Journal of Advanced Manufacturing Technology, Springer Nature
- Orientation and Supports, Carbon
- Stratasys Origin One Design Guide, Stratasys