NylonSLSHardness

Vapor Smoothing and Bead Blasting SLS Nylon Parts

Powder bed nylon is always bead blasted clean, then optionally shot surfaced for feel and color or vapor smoothed for a sealed glossy skin, and the order names the steps and the faces.

Three SLS printed nylon housings of the same design in three finishes, a raw white powder surface, an even bead blasted matte grey and a vapor smoothed black with a slight sheen.

A cube of EOS PA 2200 nylon, laser sintered on an EOS P396 and cleaned with glass beads, measured an Ra of 7.67 µm (302 µin) in a DyeMansion test. Ten minutes of shot surfacing with polymer beads at 5 bar (72.5 psi) brought it to 6.86 µm. About an hour in solvent vapor brought it to 1.89 µm (74 µin). The blasting changed the feel and the color uptake of the part more than its roughness number; the vapor changed the number by three quarters and left a different surface altogether, sealed and glossy, with marks where the part was held.

Selective laser sintering (SLS) and HP Multi Jet Fusion (MJF) build nylon parts inside a cake of powder, and every part leaves the machine with powder on its skin and a grainy surface. The finishing that follows runs in a fixed order: clean off the powder, then optionally surface by blasting, then optionally smooth by vapor or another method. Below, that order is walked step by step with the published settings and results, describe what goes wrong at each step and how it shows, and finish with what a buyer writes into the order.

The Finishing Sequence for Powder Bed Nylon

The DyeMansion test that opens this piece ran every part through the same steps, and its table of settings is the clearest published version of the sequence.

Table 1. Published finishing steps and settings for SLS and MJF nylon parts in one maker’s test
Step Machine Media Pressure or setting Duration
Cleaning, powder removal DyeMansion Powershot C Glass beads, 200 to 300 µm (0.008 to 0.012 in) 3 bar (43.5 psi) 5 min
Mechanical surfacing, PolyShot Surfacing DyeMansion Powershot S PS6 PolyBeads 5 bar (72.5 psi) 10 min
Chemical surfacing, VaporFuse Surfacing DyeMansion Powerfuse S VaporFuse VF47 Eco Fluid Vapor, then vacuum drying 45 to 57 min, by material

Source: DyeMansion, State-of-the-Art Surfacing whitepaper, 2022, Table 2. The parts were EOS PA 2200 on an EOS P396 at 120 µm (0.0047 in) layers, HP 3D High Reusability PA 12 on an HP Jet Fusion 4200 at 80 µm (0.0031 in), and a TPU on the EOS P396.

The sequence is not optional at the first step. A study of laser polishing on MJF parts, published in Lasers in Manufacturing and Materials Processing, describes depowdering with compressed air carrying glass or plastic beads as a standard step that every powder bed part needs, and notes that depending on media, pressure and time it already smooths the surface somewhat. Everything after cleaning is a choice the order makes.

Bead blasting is part of making the part. Surfacing and smoothing are finishes the drawing asks for, and each changes the part in a different way.

Step One, Depowdering by Bead Blasting

Cleaning removes loose and lightly stuck powder from every face the beads can reach. In the DyeMansion test it ran five minutes at 3 bar with glass beads of 200 to 300 µm. The laser polishing study cleaned its MJF test plates by blasting each part by hand with glass beads.

What the cleaned surface looks like depends on which side of the part it is. A University of Leeds study of PA 2200 cubes on an EOS Formiga P100 measured top and bottom faces by contact profilometry, focus variation and micro-CT, and found them distinct in both size and shape: top faces were rougher and dominated by peaks, bottom faces were neither peak nor valley dominated. Micro-CT showed that the upward-facing side of a cylinder built at 45° was less dense, more porous, than its downward-facing side. Position across the powder bed had no observable effect on roughness.

Those findings set what blasting starts from. A part’s top faces carry more and taller peaks for the beads to work on, and its up-facing sloped faces carry more porosity just under the skin.

What Goes Wrong at Cleaning

  • Powder left in blind holes, channels or under overhangs that the beads cannot reach. It shows as white residue and, later, as defects if the part goes on to vapor smoothing.
  • Fragile features damaged by the blast. DyeMansion warns that heavy parts with fragile geometries such as antennas or pins can be damaged in its shot surfacing step, and the same caution applies to any blasting of thin features.
  • Uneven cleaning inside long tubes and labyrinths, where beads lose energy after the first deflection.

Step Two, Shot Surfacing With Polymer Beads

The second step uses the same principle as cleaning with a different aim. DyeMansion describes its PolyShot Surfacing as beads accelerated by compressed air whose impact flattens peaks into valleys by plastic deformation at the microscopic scale. It contrasts this with tumbling, which removes material; in shot surfacing, it says, no material is removed and the original geometry is kept. Its Powershot S processes three quarters of an EOS P396 build or a full HP Jet Fusion 4200 or 5200 build in a 10-minute batch.

Table 2. Measured roughness of nylon parts after cleaning, shot surfacing and vapor smoothing, one maker’s test
Material and process Parameter Cleaned only Shot surfaced Vapor smoothed
EOS PA 2200, SLS Ra 7.67 µm (302 µin) 6.86 µm (270 µin) 1.89 µm (74 µin)
EOS PA 2200, SLS Sa 8.45 µm (333 µin) 7.61 µm (300 µin) 2.34 µm (92 µin)
EOS PA 2200, SLS Rz 42.2 µm (1,661 µin) 34.2 µm (1,346 µin) 11.6 µm (457 µin)
HP 3D HR PA 12, MJF Ra 9.79 µm (385 µin) 8.99 µm (354 µin) 1.60 µm (63 µin)
HP 3D HR PA 12, MJF Sa 10.8 µm (425 µin) 10.3 µm (406 µin) 1.79 µm (70 µin)
HP 3D HR PA 12, MJF Rz 50.1 µm (1,972 µin) 47.6 µm (1,874 µin) 10.2 µm (402 µin)

Source: DyeMansion, State-of-the-Art Surfacing whitepaper, Tables 3 and 4; areal values measured with a strip-light instrument as the paper describes. The column assignment follows the paper’s stated finding that vapor smoothing brings Ra below 2 µm.

Shot surfacing moves Ra by about a tenth on both processes: 7.67 to 6.86 µm on SLS, 9.79 to 8.99 µm on MJF. The paper’s own reading is that the step flattens the sharpest peaks and valleys, which it confirms with lower Sz and lower slope and developed-area parameters, so the part feels markedly smoother and takes a matte-gloss finish without the roughness average changing much. Gloss measured at 85° rose from 0.6 to 3.9 gloss units. The paper also says the step improves scratch resistance and makes the surface more resistant to dirt, and that a homogenized surface takes dye more evenly.

What Goes Wrong at Shot Surfacing

DyeMansion lists the limits. The finish varies inside thin tubes and labyrinths, out of the beads’ line of sight, which a longer cycle partly compensates. Fragile features on heavy parts can be damaged. And the process is not suited to flexible materials such as TPU, whose elastic deformation makes homogenization virtually impossible. A shot-surfaced batch with a patchy finish on its inner faces has met the first limit, not a process fault.

Shot surfacing changes the feel and the color of a nylon part far more than its Ra. A drawing that asks for a roughness number from blasting asks for the wrong thing.

Step Three, Vapor Smoothing

Vapor smoothing works by dissolving the skin rather than pressing it. DyeMansion’s description of its VaporFuse process: a polar solvent vapor condenses on the part and breaks the bonds between polymer chains at the surface; the chains rearrange to minimize surface area and energy, which smooths the surface; vacuum drying then removes the solvent and the surface solidifies in its new form. The laser polishing study describes vapor smoothing in general terms as chemical vapor that dissolves and reflows the surface layer and can smooth even partly enclosed surfaces.

The result in Table 2 is large on both processes: Ra from 7.67 to 1.89 µm on SLS and from 9.79 to 1.60 µm on MJF, and DyeMansion reports all the relevant areal parameters reduced by more than 60 %. Gloss at 85° rose from 0.6 to 24.5 gloss units. The paper describes the result as a sealed, washable surface close to an injection-molded one, achieved on complex and internal structures as well as outer faces. On a sintered TPU in the same test, Ra fell from 18.9 µm (744 µin) to 3.34 µm (131 µin). Powder makers mark the same compatibility: BASF Forward AM’s portfolio brochure lists chemical smoothing as compatible with every powder in its PP, PA11 and TPU lines.

What Goes Wrong at Vapor Smoothing

DyeMansion’s list of limits is specific, and each item shows on the part.

  1. Contact marks. The whole surface is dissolved, so marks remain where the part touched its holder. The paper suggests designing in a hook or a hanging point in the CAD file.
  2. Moving parts. The function of moving parts can be limited after vapor smoothing, since gaps between them are surfaces too.
  3. Residual powder. Powder not cleaned off in step one is dissolved and melted into the skin, so cleaning before vapor smoothing has to be thorough.
  4. Bonding and coating. A smoother surface can help or hurt later gluing or coating, case by case.

Cycle time also matters for a batch plan. The VaporFuse step in the test ran 45 to 57 minutes depending on material, against 10 minutes for shot surfacing and 5 for cleaning.

Laser Polishing as an Alternative Finish

The laser polishing study offers a third method for MJF nylon and compares it with the others. It polished HP 3D High Reusability PA 12 plates from an HP Jet Fusion 4200 with a 30 W CO2 laser and a line focus, after drying the plates at 80 °C (176 °F) for at least 2 hours to avoid blisters from absorbed water.

Table 3. Laser beam polished MJF PA 12 against the unprocessed surface, one study
Property Unprocessed Laser polished
Ra 6.4 ± 0.3 µm (252 µin) 0.6 ± 0.1 µm (24 µin)
Rq 8.1 ± 0.4 µm (319 µin) 0.8 ± 0.1 µm (31 µin)
Hardness 73 ± 3 Shore D 73 ± 3 Shore D
Tensile strength X, Y, Z 41, 44, 47 MPa (5.9, 6.4, 6.8 ksi) 39, 41, 45 MPa (5.7, 5.9, 6.5 ksi)
Water contact angle 84 ± 4° 59 ± 5°

Source: Lasers in Manufacturing and Materials Processing, 2023, Laser Beam Polishing of PA12 Parts Manufactured by Powder Bed Fusion, Table 3.

The study reports a roughness reduction of up to 91 %, an interaction time of 1.4 seconds, and a remelted depth of 100 to 400 µm (0.004 to 0.016 in) depending on time. It notes from the literature that chemically vapor-smoothed surfaces reach minimum values of Ra 0.78 µm or Sa 1.4 µm, slightly rougher than its best laser result. The trade-offs are visible in its own table: tensile strength fell slightly and the surface became more wettable. Its authors describe the method as preferable to conventional finishing in some applications, for fusing residual powder and improving tribological properties, and as still new, with the effects of its parameters not fully understood.

Measuring a Finished Nylon Surface

The numbers in Tables 2 and 3 came from different instruments and different parameters, and a finished nylon surface is easy to mis-measure. Three points from the sources decide whether a roughness value on a finished part means anything.

First, Ra alone misses what blasting does. DyeMansion argues that a two-dimensional average from a stylus cannot describe the feel and look of a finished surface, and adds areal parameters defined in ISO 25178: Sdq, the mean slope of the micro-surface, which falls as a surface looks glossier, and Sdr, the ratio of true to projected area, which falls as a surface feels smoother. Its shot-surfaced parts barely moved in Ra but dropped in both of these. A buyer who wants the feel of a shot-surfaced part and writes only an Ra limit has written a requirement that cleaning alone almost meets.

Second, the shape of the profile matters as well as its size. The Leeds study concluded that both a size descriptor and a shape descriptor are needed for laser-sintered PA12, and found Sq and Ssk, the skewness, the most appropriate pair: top faces were skewed toward peaks, bottom faces were not. Two faces with the same Sq can wear and feel differently if one is peak dominated.

Third, the method changes the number. The Leeds study measured the same surfaces by contact profilometry and by focus variation microscopy and reported the variability of each; its focus variation Sq stayed fairly constant across energy density and bed location. DyeMansion measured its areal values with a strip-light instrument and states that tactile instruments cannot give three-dimensional values. Gloss needs its own fixed angle: DyeMansion measured at 85° because the unfinished matte surface reflects too little at steeper angles to compare.

A finished nylon face is specified by the parameter that tracks the effect wanted: Ra or Sa for smoothness, a slope or gloss value for shine, and the face and method for both.

Choosing the Finish and Writing It Into the Order

The three finishes answer different needs, and the data above point to which one a part needs.

  • A clean, uniform matte part that will be dyed or painted: cleaning and shot surfacing.
  • A sealed, washable, glossy part, including internal channels and air or fluid paths, where DyeMansion notes the smooth surface reduces flow resistance: vapor smoothing, with a hanging point designed in.
  • A local smooth face, such as a sliding or sealing face, with edges and details left sharp: laser polishing, where a supplier offers it.
  • A flexible TPU part: vapor smoothing rather than shot surfacing, per DyeMansion’s limits.

The order then states the finish as a sequence and a result, not as a word.

  1. Name the finish steps: cleaned, shot surfaced, vapor smoothed or laser polished.
  2. Give the roughness requirement with its parameter, standard and the faces it applies to, after the finish.
  3. Mark where contact or hanging marks are acceptable, for vapor-smoothed parts.
  4. Mark moving assemblies and fits, and say whether they are finished assembled or apart.
  5. State that blind holes and channels are to be free of powder before smoothing.
  6. Ask for a finished sample face before the batch, since every figure here comes from one maker’s or one lab’s equipment.

For a buyer weighing low-volume 3D printing of nylon housings against molded parts for bridge production, vapor smoothing is usually the step that brings the printed surface closest to the molded one, and its hanging point is the line most often missing from the drawing.

Sources and Further Reading

Send the 3D File of Your Printed Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with 3D Printing chosen.

Request a Quote