EOS asks for a stress relief on its 316L stainless steel of at least 2 hours at 900 °C (1,652 °F) when the part is thoroughly heated, followed by a quench fast enough to stop chromium carbides forming. A cantilever printed in titanium shows why the step comes before the saw: cut free of its plate unrelieved, it bends in the plane of its length, because the top of the beam carries tension and the bottom carries compression, locked in layer by layer during the build.
Laser powder bed fusion welds metal one thin layer at a time, and each melt pool cools quickly against a solid that is already contracting. The part leaves the machine fixed to a thick plate, which holds those stresses in place. What happens between the end of the build and a part that can be measured is a sequence of heat, saw, hand work and inspection, and the order of that sequence is set by what the plate is doing.
Metal Powder Bed Fusion Post-Build Steps in Order
The post-build sequence for a part built on a plate has a stable shape across machine makers, because the stresses behave the same way. The sources agree on the order; they differ in how much of the detail they publish.
| Step | Operation | Condition and figure | Source |
|---|---|---|---|
| 1 | Stress relief, part still on the plate | typically before the part is removed from the plate | De Baere et al., Additive Manufacturing 38 |
| 2 | Cut the part from the plate | bandsaw or wire-eroding machine | MakerVerse guide |
| 3 | Remove supports | by hand, with hammer, chisel, tongs or grinders | MakerVerse guide |
| 4 | Grind the support contact surfaces | rough where each support attached | MakerVerse guide |
| 5 | Further heat treatment where properties call for it | EOS 316L solution annealing at 1,150 °C (2,102 °F) for at least 1.5 h | EOS 316L data sheet |
| 6 | Media blast | corundum, on every part in that supplier’s flow | MakerVerse guide |
| 7 | Machine critical features, if drawn | needs a drawing of the machined faces | MakerVerse guide |
| 8 | Inspect | optical 3D scan, tactile CMM, stylus roughness, CT for internal flaws | MakerVerse guide |
Steps 1 and 5 are heat treatments with different jobs. The first lowers the residual stress so that cutting will not move the part. The second changes the microstructure to reach the properties the application needs. A supplier who offers only one of them has chosen which job to do, and the buyer should know which.
The plate is a fixture. Heat first, saw second, and the part leaves the plate in the shape it was built in.
Why Parts Are Heat Treated Before They Are Cut Free
The 2021 paper by De Baere and co-authors from the Technical University of Denmark, KU Leuven and 3D Systems Leuven puts the habit in one sentence: a part made by laser powder bed fusion is typically heat treated before it is removed from the build plate. The reason is in their cantilever. The beam bends in the plane of its length after release from the plate, because the tensile residual stress at the top and the compressive stress at the bottom come out of balance once the plate stops resisting.
Heating the part relaxes the stress through two mechanisms the paper names. Raising the temperature lowers the yield strength, so the stress relaxes by plastic yielding. At higher temperatures a second mechanism, creep, adds a time-dependent reduction. The same drop in tensile stress at the surface also raises the toughness of the part.
The paper collects earlier measurements. A stress-relief treatment just below 600 °C (1,112 °F) reduced deformation from residual stress by 80 percent in one study. Neutron diffraction at 600 °C and 700 °C (1,292 °F) showed the majority of the stress gone in the first ten minutes and the stress down to a few percent after two hours, with about 90 percent gone at 600 °C after 100 minutes. A study across 427 °C to 610 °C and dwell times from 5 minutes to 30 hours found that the stresses fall quickly at first, and that some remain even at 610 °C after 30 hours. All of these are for the alloys named in those studies, mostly titanium and a stainless steel at 700 °C, and the published figures differ by source, a point the authors make themselves.
| Temperature | Dwell time | Result reported |
|---|---|---|
| just below 600 °C (1,112 °F) | not stated in the paper | deformation from residual stress reduced by 80 percent |
| 600 °C and 700 °C | first 10 min | majority of the stress relieved |
| 600 °C | 100 min | about 90 percent of the stress relieved |
| 600 °C and 700 °C | 2 h | stress down to a few percent |
| 610 °C (1,130 °F) | 30 h | some residual stress remains |
What Temperature and Time Trade Against Each Other
The paper’s own model uses a titanium alloy cantilever and plots displacement against dwell time for several temperatures. A hotter treatment relaxes the stress faster, and the authors note a process window in which the deflection after treatment is minimal. In their simulations, long holds above 750 °C stop reducing the tip deflection and increase it, because the stress redistributes and the deflection is then driven by the support rather than the beam, a result the authors say can be mistaken for incomplete relaxation. The lesson for a buyer is that time and temperature are chosen together for a given alloy and geometry, not set once for every part.
More heat does not always mean less distortion. The treatment is set for the alloy, the geometry and the supports, and a supplier should be able to say how.
The EOS 316L Figures for Heat Treatment and Build
The data sheets from a machine maker give the most specific numbers for one material. For EOS StainlessSteel 316L on the EOS M 290, the powder has a particle size distribution of 20 to 65 µm, and the data sheet lists two heat treatments.
| Item | Value | Source |
|---|---|---|
| Stress relieve | 900 °C (1,652 °F), at least 2 h when thoroughly heated, water or high-speed gas quench | EOS 316L data sheet |
| Solution annealing | 1,150 °C (2,102 °F), at least 1.5 h when thoroughly heated, water or high-speed gas quench | EOS 316L data sheet |
| Quench requirement | fast enough to prevent chromium carbide precipitation | EOS 316L data sheet |
| Typical dimensional change after heat treatment | +0.02 percent | EOS process data sheet, 40 µm |
| Layer thickness and volume rate | 40 µm at 3.7 mm3/s; 20 µm at 2.0 mm3/s | EOS process data sheets |
| Minimum wall thickness at 20 µm | 0.3 to 0.4 mm (0.012 to 0.016 in) | EOS process data sheet, 20 µm |
| Build volume | 250 × 250 × 325 mm (9.8 × 9.8 × 12.8 in) | EOS M 290 brochure |
The dimensional change of +0.02 percent after heat treatment is a small number, and it is a typical value from EOS’s own testing, so a part with a tight tolerance should still be measured after the treatment, not before. On a 100 mm (3.9 in) dimension 0.02 percent is 0.02 mm (0.0008 in). The mechanical properties as manufactured differ by direction: for the 40 µm set, EOS lists a vertical yield strength of 490 MPa and a horizontal one of 560 MPa, with tensile strengths of 600 and 690 MPa and elongation of 55 and 40 percent. A drawing for a loaded part can say which way the load runs relative to the build.
Cutting the Plate and Taking Supports Away
MakerVerse’s post-processing guide says complex components are cut from the build plate, typically with a bandsaw or a wire-eroding machine, and that this is always needed for parts with printed supports. The supports then come off by hand, using hammers, chisels, tongs or grinders, which the guide calls time-consuming and labor-intensive. The areas where supports attached are rough and are smoothed by hand.
Support removal is therefore both a cost and a source of variation. Each support contact is a place where a tool can mark or move a thin feature. The sources do not give a time per support or a roughness figure for the contact faces, so a buyer who needs either should ask the supplier for measured values from its own parts, with the measurement method named.
The same guide treats the heat treatment as optional but recommended: printing induces internal stress, which can cause deviations or, in the worst case, part failure, and the treatment can come at completion or before other post-processing. The guide gives no temperatures. Where a drawing calls for high strength and low elongation, such as a tool steel part, the guide says the treatment is needed.
Where the Plate Itself Fits
The plate is part of the process, not an afterthought. It is the thing that carries heat out of the first layers, and it stays bolted to the part through the heat treatment in the order above. For that reason a supplier’s quotation for a metal part should show the plate step as a named operation, with its method, rather than leaving it inside a lump called finishing.
How Long the Build Takes Before Any of This Starts
The heat treatment and the saw come after a build whose length the machine maker also publishes. EOS gives a volume rate for each parameter set: 3.7 mm3/s for 316L at 40 µm and 8.4 mm3/s at 80 µm, with the note that the rate depends on part dimensions and skin thickness. The 20 µm set is 2.0 mm3/s. The M 290 carries a 400 W fiber laser and runs under argon or nitrogen, and its monitoring records laser power across the build and images the powder bed after each recoat and exposure.
The volume rate converts to time by plain division. At 3.7 mm3/s, one cubic centimeter of solid (1,000 mm3) takes about 270 seconds of exposure, so a 100 cm3 part needs roughly 7.5 hours of exposure at 40 µm and about 3.3 hours at 80 µm. This is arithmetic from the published rates, it leaves out recoating time and the plate’s warm-up, and the sheet’s own caveat about part dimensions applies, so it sizes a build rather than predicting one.
Two consequences matter for a plan. The thicker layer option shortens the build at a cost to the fine detail that the 40 µm set is described as giving, and the maker says the 40/80 µm skin option can cut total build time at the same surface quality by assigning layer thickness to different regions of the part. And the heat treatment adds its own hours to the calendar: at least 2 hours at 900 °C for the stress relief alone, before the furnace’s heating and cooling time, which the data sheet does not state.
What Goes Wrong Between the Build and the Part
The failures in this sequence are mostly dimensional, and they are seen on a measuring machine.
- A part that is out of flat by an amount larger than the drawing allows after it is cut from the plate: stress that was not relieved first.
- A stainless part whose corrosion resistance or properties are off: a quench slower than the data sheet’s requirement, which allows chromium carbides to form.
- A thin feature that moved or marked when its support was pulled: EOS gives 0.3 to 0.4 mm (0.012 to 0.016 in) as the minimum wall at 20 µm, and a wall near that size has little margin against a chisel.
- Properties that differ from the data sheet by direction: loads along the build axis against loads across it, where EOS’s own figures differ by 70 MPa in yield strength.
MakerVerse names four inspection methods for metal parts.
- Optical 3D scan, the fastest, which compares overall form against the model.
- Tactile CMM, slower and more precise, for datum and feature dimensions.
- Stylus measurement of surface roughness.
- Computed tomography, which finds internal pores, inclusions and voids.
EOS’s process data sheet reports defect percentage and density by sample count: 0.018 percent average defects across 45 samples and a density of at least 7.97 g/cm3 for the 20 µm set. The figures are statistics of EOS’s own validation builds, and EOS notes that tolerance intervals are based on validation data and are not directly transferable to other systems.
What to Write Into an Order for a Metal Printed Part
ISO/ASTM 52901:2017 sets out what a buyer and a part provider exchange at the time of the order: the part definition and geometry, tolerances, surface texture, the manufacturing process, the feedstock, repair methods, acceptable imperfections, process control information and authorized outside service providers, then characteristics, inspection and post-processing, then acceptance. Each item of the sequence in Table 1 has a place.
- Heat treatment before plate removal, with the method named rather than the temperature alone.
- The cutting method, saw or wire erosion.
- The support removal method and which faces may carry marks.
- The inspection method for each critical dimension, and when it is made, before or after heat treatment.
- Acceptance of a first production part before the run, since the standard has a clause for it.
An order that names those five items is the one that gets a part that holds its shape from the plate to the gauge, and it is the order a buyer of low-volume 3D printing should place when the same metal part will repeat in bridge production.
Sources and Further Reading
- D. De Baere, P. Van Cauwenbergh, M. Bayat, S. Mohanty, J. Thorborg, L. Thijs, B. Van Hooreweder, K. Vanmeensel, J. H. Hattel, Thermo-mechanical modelling of stress relief heat treatments after laser-based powder bed fusion, Additive Manufacturing 38 (2021) 101818, Technical University of Denmark repository
- EOS, EOS StainlessSteel 316L material data sheet
- EOS, Process data sheet, EOS StainlessSteel 316L-4404 for EOS M 290, 40 µm
- EOS, EOS M 290 brochure, additive manufacturing system for serial components, spare parts and functional prototypes
- MakerVerse, The guide to laser powder bed fusion (LPBF) post-processing
- ISO and ASTM, ISO/ASTM 52901:2017, requirements for purchased AM parts