Over seven laser sintering builds with nylon 12 powder refreshed at 30 % virgin material after each one, a University of Birmingham study measured part porosity rising by 5.8 % and tensile strength falling by 11 %. No single build failed. The parts of the seventh build were simply weaker than the parts of the first, and the cause was in the powder, not in any one print. A defect in a production batch is read by its pattern: whether it appears in every part, in one zone of the build, in one build only, or a little more in each build than the last.
The sections below sort the defects of powder bed printing, polymer and metal, by that pattern. Each pattern points to a different cause, a different piece of evidence and a different fix, and a buyer who knows which pattern a reject belongs to knows which question to ask the supplier. Two reviews carry most of the metal side: a NIST literature review of metal AM defects and a 2022 review of defects and anomalies in powder bed fusion by Mostafaei and co-authors. Three studies of nylon powder reuse carry the polymer side.
Reading a Defect by Its Pattern Across the Batch
The 2022 review sorts the sources of metal powder bed defects into three groups: defects transferred from the feedstock powder, defects formed in the interaction of the beam with powder and metal during melting, and defects created in post-processing such as heat treatment. It adds a fourth set of contributors around them: the equipment, powder handling and dispensing, and build preparation, meaning orientation and supports. Each source leaves a different footprint in a batch.
| Pattern in the batch | Typical defects | Cause the sources point to | Evidence to ask for |
|---|---|---|---|
| Every part, every build | Lack-of-fusion or keyhole porosity, low elongation | Parameter set outside the process window | Parameter set, density coupons, CT of a sample |
| One zone of the platform | Porosity, spattered powder, poor size, rough surfaces | Gas flow and spatter redeposition near the outlet; beam distortion at high deflection angles | Build layout with positions, reject map by position |
| One build only | Streaks, short layers, deformed parts | Recoater damage, a spatter particle hit by the blade, a powder lot | Build log, layer images, powder lot record |
| Worse in each build | Higher porosity, lower strength, more shrink, rougher skin | Powder aging from reuse | Refresh ratio, build count of the powder, powder tests |
| After heat treatment | Pores reappearing after HIP and a later anneal | Argon in pores regrowing | Thermal history, order of HIP and heat treatment |
Sources: Mostafaei and co-authors, Defects and anomalies in powder bed fusion metal additive manufacturing, 2022, sections 1.4 and 4; Kim and Moylan, NIST AMS 100-16; University of Birmingham and Staffordshire University studies on PA12 reuse.
A reject is half a diagnosis. The other half is where in the build it sat and which build of the batch it came from.
Porosity in Every Part From the Parameter Set
The most common defects in metal powder bed fusion are processing defects, and porosity leads them. NIST’s review divides it into two kinds. Lack-of-fusion porosity comes from a poor choice of processing parameters and leaves pores of irregular shape along the hatch tracks or between layers. Gas porosity leaves spherical pores from gas trapped in the powder particles or from the shielding gas during melting, and is harder to eliminate; the review cites one study where it reached 0.7 %. Both kinds can sit in the same part. One study in the review found a gas pore of about 80 µm (0.003 in) diameter beside an irregular lack-of-fusion pore of about 400 µm (0.016 in).
The 2022 review adds a third kind and draws the window between them. Lack of fusion sits on one side, where melt pools do not overlap enough to melt every point at least once. Keyhole porosity sits on the other, where a deep vapor cavity in the melt pool becomes unstable and pinches off pores. A beading-up boundary, set by fluid flow and capillary instability, limits how fast and hot the process can run. Inside the window parts reach nominally full density, which the review quantifies as more than 99.9 % by volume, though it warns that large defects are still possible inside the window and that standard recommended settings can still give keyhole or lack-of-fusion pores.
| Type | Shape | Origin | Example from the reviews |
|---|---|---|---|
| Lack of fusion | Irregular, along tracks or between layers | Too little melt pool overlap; poor parameters | About 400 µm (0.016 in) in one study |
| Gas porosity | Spherical | Gas in atomized powder or shielding gas | About 80 µm (0.003 in); up to 0.7 % in one study |
| Keyhole | Rounded, often deep in the track | Unstable deep vapor cavity in high-energy melting | Boundary drawn in power and speed space |
| Balling or bead-up | Uneven tracks, voids | Capillary instability; high chamber oxygen promotes it | Limits faster, hotter settings |
Sources: Kim and Moylan, NIST AMS 100-16, Porosity section; Mostafaei and co-authors, 2022, sections 1.4.1 and 4.
A pattern of the same pore type in every part of every build is the signature of the parameter set. NIST cites a study in which the best hatch spacing, about 120 µm (0.005 in) for a 70 µm laser spot, matched the real width of a track; a spacing far from it left pores between tracks in every layer. The fix is in the parameters, and the evidence is density coupons and computed tomography (CT) of parts from more than one build.
Why the Size of a Pore Matters More Than the Total
A 2020 review from Penn State in Additive Manufacturing states that it is widely accepted that gas porosity and lack-of-fusion flaws degrade both static and dynamic performance, while the mechanisms by which they form are still debated and their effect on dynamic performance is not yet fully quantified.
NIST notes that overall porosity of about 1 to 5 % is now typical for some materials after optimization, and that a low total can still hide a single pore large enough to start a failure. It cites fatigue tests in which internal defects of 500 µm (0.020 in) or larger sharply reduced the cycles to failure, and in which hot isostatic pressing improved fatigue strength. A separate study of laser-melted 316L found pores above 125 µm (0.005 in) diameter to be the threshold that best predicted the loss of ductility. Any batch acceptance criterion written as a total porosity percentage misses the defect that breaks the part.
Defects in One Zone of the Platform
When rejects cluster by position, the cause is the machine and its environment rather than the parameters. The 2022 review lists the mechanisms.
- Gas flow. An inert gas flows over the build surface, and its rate and path decide where spatter lands; redeposited spatter near the gas outlet causes porosity, spattered powder, poor dimensional accuracy and rough surfaces. Higher gas velocity increased powder bed contamination in one study it cites.
- Spatter on the bed. Spattered particles are usually coarse, so a beam passing over one may not melt it fully, leaving a pore.
- Beam geometry. The laser or electron beam can distort elliptically near the edge of the plate because of high scanner deflection angles, which by position can cause lack of fusion or poor geometry.
- Calibration. An incorrectly calibrated system can produce geometric inaccuracy, and the quality of optics alignment, mirrors and beam profile all affect the process.
Polymer builds show position effects of their own. A 3D Systems ProX SLS 6100 study of 50 nylon 12 parts in three zones found positional deviations grow by up to 0.1 mm (0.004 in) toward the edges of the platform. Colibrium Additive publishes a platform stability build for 316L across 16 positions precisely because position is a variable a buyer can ask about.
A reject map that records each part’s position in the build is the evidence that separates a zone effect from a parameter effect.
Defects in One Build of the Batch
A defect that appears in one build and not in the next points to an event during that build. The 2022 review names the recoater as a common one. A recoater can leave a powder layer uneven in density and smoothness; a spatter particle on the solid area can be struck by the blade, deforming the part and leaving an anomaly in the next spread layer. An uneven layer changes the laser and powder interaction and can form porosity. Rubber or brush recoaters reduce collisions and friction but are damaged more easily and replaced more often.
The same review lists what in-process monitoring watches for in the powder layer: defective spread layers, unevenness from part distortion, incomplete spreading, recoater hopping and recoater streaking. Those words describe what a layer image from a failed build shows. The baseplate matters too: warping, deformation, layer delamination and cracking all depend on it, along with print strategy and laser power, and its thickness changes heat dissipation and thermal stress.
A one-build defect is an event, and the build log is where it was recorded. A supplier who keeps layer images can show the layer where it began.
A New Powder Lot as the Event
A change of metal powder lot is the other one-build event. The 2022 review ties powder-related defects to morphology, flowability, mean size and size distribution, and surface contamination, all set by how the powder was made. Spherical powder packs and flows better; very fine particles under 5 µm (0.0002 in) can agglomerate and lower packing and part density. It gives 15 to 45 µm as the typical size range for laser powder bed fusion and 45 to 110 µm for electron beam machines, with the layer thickness chosen from the powder’s size. Moisture, organic contamination and gas trapped inside particles all carry into the part. A defect that starts with the first build on a new lot points to the powder certificate before the machine.
Residual Stress and Cracking
Some defects belong to the part’s own geometry and show in every build of that part. NIST cites measurements of residual stress up to 500 MPa (72.5 ksi) in the top layer of a laser-built steel part, relieved by heating above 600 °C (1,112 °F) for an hour, and reduced by rescanning or by heating the base plate. The 2022 review notes that cracking, distortion and super-elevated edges follow the thermal history and print pattern, which scan strategy and part design control, and that low heat input reduces thermal strain. A crack that recurs at the same feature in every build is a design or strategy problem, not a lot problem.
Defects That Grow Build by Build From Powder Reuse
In polymer powder bed fusion the most important batch-level defect is gradual. Unfused powder is reused, and it ages each time it is heated. A study in the Journal of Manufacturing Processes on nylon 12 from an EOS P 390 describes two kinds of change: reversible physical change, such as post-crystallization and agglomeration, and irreversible chemical degradation by thermal oxidation and post-condensation, which changes molecular weight, flowability and melt viscosity. It also separates powder by where it sat: powder far from the parts, reused in practice, and extremely aged powder close to the heat-affected zones around parts, which is not usually reused.
| Study | Reuse scheme | Change in powder | Change in parts |
|---|---|---|---|
| University of Birmingham, Additive Manufacturing 80 | 70:30 used to virgin, seven builds | Melting temperature up 4.5 °C (8.1 °F); flowability down 20 % | Porosity up 5.8 %; tensile strength down 11 % |
| Staffordshire University, Additive Manufacturing Frontiers 4, 2025 | Six iterations of reuse | Agglomerated particles under 10 µm (0.0004 in) not present in virgin powder | Shrinkage up by 0.98 % absolute, 30.63 % relative, on a 3.2 % baseline; small rise in elongation at yield and in tensile strength |
| Journal of Manufacturing Processes study | Interlayer heating with up to 30 % extremely aged powder | Process control compensates aging | 18.04 % higher tensile strength and 55.29 % higher elongation than its benchmark |
Sources: the three papers named in the first column.
The Birmingham study found the loss of flowability the most significant cause of the loss of strength, with a p-value of 0.005, and pointed to the powder flow test it used as a practical check on used powder. Staffordshire’s study notes that suppliers recommend reusing 50 to 70 % of reprocessed powder, and its main finding for a buyer is dimensional: reuse changed shrinkage enough to move part size. Sinterit, a powder and machine maker, writes the same drift into its datasheet for its Flexa TPU: an extra 50 % refresh may be needed when surface quality drops, which it says can happen every few to more than a dozen prints.
The signature in a batch is a trend: porosity, strength, size or surface moving in one direction across builds while each build looks normal. Evidence for it is the powder record: refresh ratio, number of cycles, and a flow or melting test on the powder going into each build.
Defects Created After Printing
Post-processing can repair defects and create new ones. The 2022 review describes hot isostatic pressing as the frequent cure for internal porosity, shrinking pores under heat and pressure and improving elongation and fatigue life, at the cost of microstructural coarsening and some strength. It then names the trap: pores holding argon, closed by HIP, can regrow during a later high-temperature heat treatment, a process known as thermally induced porosity, sometimes enough to degrade properties. Keyhole and lack-of-fusion pores could feasibly contain shielding gas. A batch whose CT was clean after HIP and whose parts lost ductility after a later anneal has met this mechanism, and the order of thermal steps is the evidence.
Inspection Plan for a Powder Bed Batch
The patterns above lead to an inspection plan that finds the cause, not only the reject.
- Record each part’s build number and position, so rejects can be mapped by zone and by build.
- Print density or tensile coupons in every build, at more than one position, so a parameter drift and a zone effect can be told apart.
- Sample parts for CT where internal defects matter. NIST calls CT a promising technique for porosity while noting that critical defect criteria by type, size, orientation and distribution are yet to be settled, so the acceptance limit is agreed per part.
- State acceptance limits by largest pore size, not only by total porosity.
- Keep the powder record for polymer and metal builds: lot, refresh ratio, cycle count and a flow test.
- Ask for layer images or monitoring data where the supplier’s machine records them.
- Record the order and conditions of HIP and heat treatment for metal parts.
For a buyer running low-volume 3D printing across many builds for bridge production, the build number and position written on every part are what turn a pile of rejects into a cause that can be fixed before the next build starts.
Sources and Further Reading
- Literature Review of Metal Additive Manufacturing Defects, NIST AMS 100-16, May 2018, National Institute of Standards and Technology
- Defects and anomalies in powder bed fusion metal additive manufacturing, Current Opinion in Solid State and Materials Science 26, 2022, via NSF Public Access Repository
- Invited Review Article, Review of the formation and impact of flaws in powder bed fusion additive manufacturing, Additive Manufacturing 36, 2020, Penn State
- Re-use of polyamide-12 in powder bed fusion and its effect on process-relevant powder characteristics and final part properties, Additive Manufacturing 80, University of Birmingham
- Aging dynamics in polymer powder bed fusion systems, the case of selective laser sintering, Additive Manufacturing Frontiers 4, 2025, Staffordshire University
- A process control and interlayer heating approach to reuse polyamide 12 powders and create parts with improved mechanical properties in selective laser sintering, Journal of Manufacturing Processes, via NSF Public Access Repository
- Effects of Spatial Energy Distribution-Induced Porosity on Mechanical Properties of Laser Powder Bed Fusion 316L Stainless Steel, Georgia Institute of Technology and Sandia National Laboratories via NSF PAR
- Influence of part orientation and spatial placement on the dimensional and surface quality of SLS-printed PA12 components, Springer Nature
- Flexa Performance, Material’s Technical Data Sheet, Sinterit
- L-PBF Stainless Steel 316L Parameters for M2 Series 5, Colibrium Additive