Formlabs prints two numbers for its Tough 2000 resin next to extruded ABS sheet and they point in opposite directions. Both materials show a tensile modulus of 1,800 MPa (261 ksi), and the printed resin stretches 79 % before it breaks where the ABS stretches 8 %. On the energy to fracture the order flips: 305 J/m² for the resin against 2,060 J/m² for the ABS. The resin is stiffer than its elongation suggests, tougher than its modulus suggests, and a long way from the plastic it is named after in one row of the table.
Resin makers sell “tough”, “durable” and “PP-like” grades for stereolithography (SLA) as stand-ins for the thermoplastics a molded part would use. The comparison is useful and it is partial. The sections below set the published figures of four grades side by side, mark the rows where the stand-in and its model part ways, and list the questions a buyer asks before a printed part replaces a molded or machined one.
What a Tough SLA Resin Is Meant to Replace
A tough SLA resin is a photopolymer that cures under ultraviolet light into a solid that bends before it breaks. Its makers aim it at the parts where earlier SLA resins cracked: snap fits, hinges, housings that are dropped and jigs that get clamped. 3D Systems describes Accura Xtreme as a grey plastic with the durability to replace CNC-machined polypropylene and ABS articles, and Accura 25 as a white resin to simulate machined polypropylene. Formlabs benchmarks Tough 1000 against HDPE, Tough 1500 V2 against polypropylene and Tough 2000 V2 against ABS. Stratasys sells Somos EvoLVe 128 for tough, functional prototypes, snap-fit designs and jigs.
The word that matters in each of those lines is “against”. A benchmark names the thermoplastic a resin resembles in one or two rows, usually stiffness and strength. It does not claim the two share a failure mode, a creep curve or a temperature limit.
A tough SLA resin matches its thermoplastic on the rows its maker chose to print. The rows left out of the comparison decide whether the part survives.
Two of the four resins on these pages are also sold as master patterns for casting. Accura 25 lists master patterns for vacuum casting and Accura Xtreme lists master patterns for RTV and silicone molding among their applications. That use depends on surface and size, not on elongation, and it is a reason a buyer may order the same resin for a different job than the one its mechanical row suggests.
Tough SLA Resin Properties Compared
Table 1 gives the mechanical rows the datasheets share. Every figure is for post-cured material, and every maker states its own conditions, so the table keeps them in the notes.
| Property | Accura Xtreme (large frame SLA) | Accura 25 | Formlabs Tough 2000 V2 | Somos EvoLVe 128 |
|---|---|---|---|---|
| Tensile strength | 38 to 44 MPa (5.5 to 6.4 ksi) | 38 MPa (5.5 ksi) | 40.4 MPa (5.9 ksi) | 56.8 MPa (8.2 ksi), at yield |
| Tensile modulus | 1,790 to 1,980 MPa (260 to 287 ksi) | 1,590 to 1,660 MPa (230 to 240 ksi) | 1,800 MPa (261 ksi) | 2,964 MPa (430 ksi) |
| Elongation at break | 14 to 22 % | 13 to 20 % | 79 % | 11 % |
| Flexural strength | 52 to 71 MPa (7.5 to 10.3 ksi) | 55 to 58 MPa (8.0 to 8.4 ksi) | 67 MPa (9.7 ksi) | not published |
| Flexural modulus | 1,520 to 2,070 MPa (220 to 300 ksi) | 1,380 to 1,660 MPa (200 to 240 ksi) | 1,701 MPa (247 ksi) | 2,654 MPa (385 ksi) |
| Notched Izod impact | 35 to 52 J/m (0.7 to 1.0 ft-lb/in) | 19 to 24 J/m (0.4 ft-lb/in) | 25 J/m | 38.9 J/m (0.729 ft-lb/in) |
| Shore D hardness | 86 | 80 | not published | 82 |
| Water absorption | not published | not published | not published | 0.4 % (ASTM D570) |
Sources: 3D Systems data sheets for Accura Xtreme and Accura 25 (September 2020), tested to ASTM D638, D790 and D256; Formlabs Tough 2000 Resin V2 page, parts printed at 100 µm on a Form 4 and post-cured for 12 minutes at 70 °C in a Form Cure V2, test standards not stated on the page; Stratasys data sheet for Somos EvoLVe 128 (January 2023), UV post-cure, ASTM D638M, D790 and D256A.
The table has three readings.
- Stiffness divides the field. EvoLVe 128 is 50 to 86 % stiffer than the others on tensile modulus (2,964 MPa against a range of 1,590 to 1,980 MPa) and it breaks at 11 % elongation.
- Elongation divides it again, in the other direction. Tough 2000 V2 stretches 79 % where Accura Xtreme stretches 14 to 22 %, a ratio of about 3.6 to 5.6.
- Impact does not follow elongation. Accura Xtreme, with a quarter of the stretch, records a notched Izod of 35 to 52 J/m against 25 J/m for Tough 2000 V2. The sheets do not state the Formlabs test standard, so the two Izod figures may not come from the same procedure, and a buyer who sees them side by side should ask.
Notched impact measures how a part behaves with a sharp notch in it, such as a molded-in corner or a layer line. Elongation measures what the bulk does when it is pulled slowly. A part with a thin hinge cares about the second, and a part with a sharp inside corner cares about the first.
Thermal Limits Sit Below the ABS They Imitate
Heat is where the stand-in loses its argument. Table 2 sets the thermal rows against what Formlabs prints for ABS.
| Property | Accura Xtreme | Accura 25 | Tough 2000 V2 | EvoLVe 128 | ABS (literature value quoted by Formlabs) |
|---|---|---|---|---|---|
| HDT at 0.45 MPa | 62 °C (144 °F) | 58 to 63 °C (136 to 145 °F) | 70 °C (158 °F) | 52.3 °C (126 °F), at 0.46 MPa | about 80 to 90 °C (176 to 194 °F) |
| HDT at 1.8 MPa | 54 °C (129 °F) | 51 to 55 °C (124 to 131 °F) | 57 °C (135 °F) | 49.6 °C (121 °F), at 1.81 MPa | not stated |
| Glass transition (DMA) | 70 to 74 °C large frame, 52 °C ProJet | 72 to 74 °C (162 to 165 °F) | not published | not published | not stated |
| Thermal expansion | not published | 107 × 10⁻⁶ per °C below Tg, 151 × 10⁻⁶ per °C at 75 to 140 °C | 134.2 µm/m/°C | 56.5 to 174 µm/m/°C by range, −40 to 150 °C | not stated |
Sources: the four data sheets named under Table 1 and the Formlabs Tough 2000 V2 comparison table, which gives the ABS range as “from literature”.
The loaded heat deflection temperature (HDT) at 1.8 MPa sits between 49.6 and 57 °C on every resin in the table. A housing near a motor or a bracket in a sunlit enclosure can reach that level, and the resin then deflects under its own load long before the polymer softens in any other sense. Tough 2000 V2 at 70 °C and 0.45 MPa is 10 to 20 °C below the ABS range Formlabs quotes, and the page says so openly.
Accura Xtreme appears twice in the thermal row because 3D Systems prints two columns for it. The large frame SLA printers give a glass transition of 70 to 74 °C and the ProJet printers 52 °C, with the same HDT values in both. The same resin name covers different cured materials on different machines, and the order should name the printer family as well.
EvoLVe 128 gives its thermal expansion as a coefficient that climbs with temperature: 56.5 µm/m·°C from −40 to 0 °C, 76.5 from 0 to 50 °C, 163 from 50 to 100 °C and 174 from 100 to 150 °C. A part that is dimensionally fine at room temperature grows about twice as fast per degree once it passes 50 °C. A 100 mm dimension heated from 50 to 100 °C grows by roughly 163 × 10⁻⁶ × 50 × 100 mm, which is 0.8 mm (0.03 in).
Elongation, Fracture Energy and the ABS-Like Label
Formlabs puts its own resin and extruded ABS in one table, which is the most open comparison among the four makers, and the result is mixed.
| Property | Tough 2000 V2 | ABS sheet | Resin as share of ABS |
|---|---|---|---|
| Ultimate tensile strength | 40.4 MPa (5.9 ksi) | 39 MPa (5.7 ksi) | 104 % |
| Tensile modulus | 1,800 MPa (261 ksi) | 1,800 MPa (261 ksi) | 100 % |
| Elongation at break | 79 % | 8 % | about 10 times |
| Gardner impact at 0.8 mm | 1.6 J (14 in-lb) | 2.3 J (20 in-lb) | 70 % |
| Work of fracture | 305 J/m² | 2,060 J/m² | 15 % |
| HDT at 0.45 MPa | 70 °C (158 °F) | about 80 to 90 °C from literature | 10 to 20 °C lower |
Source: Formlabs, Tough 2000 Resin V2 product page, mechanical properties table. The page prints 4,351 psi next to the 39 MPa of ABS; the conversion from MPa used here is the arithmetic value of 5.7 ksi.
Strength and stiffness match. The energy the resin absorbs before it fails is 15 % of the ABS figure, and the Gardner impact test at 0.8 mm thickness gives 70 % of the ABS result. Formlabs notes on the same page a creep strain of only 1.3 % under a 4 MPa load after two weeks, which is the figure a jig or a clamped enclosure reads.
An engineer reading “ABS-like” therefore reads two rows as matched, one as far higher (elongation), and three (drop impact, fracture work and heat) as lower. Whether that matters depends on the part, so the list below sorts typical uses by the row that governs them.
- A snap fit that flexes once at assembly leans on elongation, where the resin is far ahead.
- A housing that is dropped leans on the work of fracture and impact rows, where the resin is behind the ABS it copies.
- A clamp or jig that carries a steady load leans on creep and loaded HDT, where Tough 2000 V2 has published figures and the other grades have none.
“ABS-like” is a statement about two rows of a data table. The fracture row and the heat row belong to the part’s actual duty.
Post-Cure, Green State and the Dimension You Ordered
Every figure above is a post-cured figure. The Formlabs page states it directly: post-curing completes the chemical reaction started during printing and takes the part from its green state to its finished properties. Formlabs gives its own conditions, 12 minutes at 70 °C in a Form Cure V2, and every maker’s number belongs to its own wash and cure schedule.
Post-cure also changes size. The Formlabs tolerance guide states that post-curing causes shrinkage in SLA and DLP parts, that it is normal for the process, and that the company’s print preparation software compensates for it automatically. The same guide gives the tolerance Formlabs expects from SLA and DLP: ±0.15 % for features of 1 to 30 mm, ±0.2 % for 31 to 80 mm and ±0.3 % for 81 to 150 mm, with a lower limit of ±0.02 mm.
For the 3D Systems resins the printer’s own data matter. The SLA 750 specification lists dimensional tolerances of ±0.051 mm for sizes below 34 mm and 0.15 % cumulatively beyond 34 mm, so a 100 mm dimension carries about ±0.15 mm. A tough resin does not change those printer-side figures, though a resin with a high green modulus holds thin features better during the print.
Liquid Properties Belong to the Machine
The datasheets also print liquid and optical rows: viscosity of 225 cps for Accura Xtreme, 230 cps for Accura 25 and about 380 cps for EvoLVe 128, all at 30 °C, and cure parameters such as penetration depth (4.1, 4.2 and 4.3 mils, or about 0.10 to 0.11 mm) and critical exposure (11.7, 10.5 and 9.3 mJ/cm²). They tell the printer operator how the resin cures. A buyer has no use for them, and no row in the cured table depends on them alone.
Choosing Between a Tough Resin and the Thermoplastic Itself
A tough resin earns its place in three cases. The part may be a first article or a pilot lot, where the material is a question a printed part can answer without a tool. The shape may be impossible to machine or mold without a split, such as an enclosed channel or an undercut that would need side actions. Or the part may be a master for a silicone tool, where the finish and the size matter and the mechanical row does not.
It does not earn the place when the part will see sustained heat above about 50 °C under load, repeated impact on a sharp corner, long outdoor exposure or a regulated use that the resin’s maker has not declared for the grade. The sheets state that values vary with machine, processing and post-cure practice, and the declarations for any specific use sit with the part’s maker.
What to Write Into the Order
- Name the resin, the printer family, the layer thickness and the post-cure schedule, in the maker’s words.
- Ask for the property that governs the duty, and the standard it was tested to: elongation, notched Izod, work of fracture, loaded HDT or creep.
- Ask for the build orientation, because the Formlabs page states that properties vary with geometry, orientation, print settings and temperature.
- State the dimension basis: after post-cure, in millimeters, with the tolerance written as a percentage and a floor, as the SLA makers write theirs.
- Write whether a printed witness bar goes with the lot, and who tests it.
Once the lines above are written into the order, a buyer comparing low-volume 3D printing in a tough resin against a molded tool for bridge production is comparing two sets of conditions and not two brand names.
Sources and Further Reading
- 3D Systems, Accura Xtreme data sheet, Tough/Durable Class, 09-20. https://www.3dsystems.com/materials/accura-xtreme
- 3D Systems, Accura 25 data sheet, PP Class, 09-20. https://www.3dsystems.com/materials/accura-25-sla
- 3D Systems, SLA 750 product page, accuracy specification. https://www.3dsystems.com/3d-printers/sla-750
- 3D Systems, Accura Materials Selection Guide for Stereolithography (SLA). https://www.3dsystems.com/materials
- Formlabs, Tough 2000 Resin V2 product page, mechanical properties and ABS comparison. https://formlabs.com/products/tough-2000-resin/
- Formlabs, Guide to 3D Printing Tolerances, Accuracy, and Precision, 12 May 2023. https://formlabs.com/blog/understanding-accuracy-precision-tolerance-in-3d-printing/
- Stratasys, Somos EvoLVe 128 data sheet MDS_SL_Somos EvoLVe128_0123a. https://www.stratasys.com/en/materials/materials-catalog/stereolithography-materials/somos-evolve-128/