The same small 3D printed test block made four ways, clear SLA resin with a smooth face, white SLS nylon with a grainy face, dark grey MJF nylon and matte grey metal with a rough as-printed face.

On an SLA test part in Accura ClearVue printed on a ProJet 6000 HD, the face built flat measured an Ra of 1.733 µm (68 µin), the face built at 30° measured 2.686 µm (106 µin) and the vertical face 1.649 µm (65 µin). A laser-sintered PA12 part from an EOS Formiga P100 gave an areal roughness Sa of 27.86 µm (1,097 µin) that barely moved with the angle at all. The first process makes roughness a question of how the part is turned in the machine. SLS makes it a property of the process, and turning the part changes little.

The sections below set out the published roughness of the common printing processes, then take orientation face by face for resin, powder bed polymers and metals, read how the numbers were measured, and end with how a roughness requirement is written on the drawing of a printed part. Every figure carries its machine, material and method, because roughness from one study does not carry over to another without them.

Typical Ra and Sa of SLA, SLS, MJF and Metal Surfaces

A review of as-printed polymer roughness in the International Journal of Advanced Manufacturing Technology collects dozens of studies by process. Another study printed one test artifact on four processes and measured them all the same way. Read together with makers’ metal datasheets, they give the ranges in Table 1.

Table 1. Published as-printed roughness by process, with machine, material and measurement
Process and material Machine Value Surface and method
SLA, Accura ClearVue 3D Systems ProJet 6000 HD Ra 1.2 to 3.4 µm (47 to 134 µin) All build angles, non-contact profilometry
SLA, Watershed 1120 3D Systems Viper SI2 Ra 1.2 µm contact, 1.0 µm non-contact (47 and 39 µin) 0.1 mm layers
Masked SLA, acrylic resins Phrozen Sonik Mini 4K Sa 6.72 to 8.54 µm (265 to 336 µin) 0.05 mm layers, optical on silicone replicas
Material jetting, VeroClear Stratasys Eden 260V Sa 11.65 µm (459 µin) 0.032 mm layers, optical on replicas
SLS, PA2200 nylon 12 EOS Formiga P100 Sa 27.86 µm (1,097 µin) 0.1 mm layers, optical on replicas
SLS, PA12 EOS P396 Ra 13.4 µm (528 µin) Contact profilometry
MJF, PA12 HP Multi Jet Fusion 4200 Ra 11.9 µm (469 µin) Contact profilometry, 20 % new powder
MJF, PA12 HP Multi Jet Fusion 4200 Ra about 15.58 µm top, 6.31 µm bottom (613 and 248 µin) 0.08 mm layers, contact profilometry
LPBF, 316L Nikon SLM 280, 30 µm Ra mean 6 µm, maximum 12 µm (236 and 472 µin) As built, 95/95 maximum
LPBF, AlSi10Mg AddUp FormUp 350, 50 µm Ra 6 to 8 µm (236 to 315 µin) Vertical, optical, cutoff 2.5 mm
LPBF, AlSi10Mg Gränges sheet, 50 µm Ra 11 to 20 µm (433 to 787 µin) Vertical, DIN ISO 13565-1 and -2

Sources: Golhin and co-authors, Surface roughness of as-printed polymers, Tables 9 to 11; the multi-process orientation study in PMC; Nikon SLM Solutions, AddUp and Gränges datasheets.

Three readings come out of the table. Vat photopolymerization with a laser gives the smoothest as-printed faces, around 1 to 3 µm Ra on most faces. Powder bed polymers, laser-sintered or MJF, sit around 12 to 15 µm Ra on most faces, roughly five to ten times rougher, because fused grains and partly melted particles stay on the skin. Metal LPBF sits between the two, and differs widely between makers’ sheets even for one alloy, as the two AlSi10Mg rows show.

Ra and Sa are not the same number. Of the two, Ra is the average height of a single traced profile; Sa is the same average over an area. A buyer who compares an Sa from one study with an Ra from another is comparing two measurements, and the table keeps them in separate words for that reason.

Process sets the floor of roughness. SLA starts near 1 µm Ra, a powder bed near 12 µm, and no orientation choice in a powder bed brings it near the resin figure.

Build Angle and the Staircase on Sloped Faces

Every printed part is a stack of layers, and a sloped face is a staircase whose step height is the layer thickness. The steps are what orientation changes. In resin processes, which have little roughness of their own, the staircase is most of what there is to measure.

SLA Faces by Angle

The review lists SLA studies that varied the build angle and measured each face.

Table 2. Roughness against build angle in published SLA and LPBF studies
Study, machine and material Flat or 0° 30° to 45° Vertical or 90° Method
SLA, ProJet 6000 HD, Accura ClearVue Ra 1.733 µm (68 µin) 2.686 µm at 30°, 2.546 µm at 60° 1.649 µm (65 µin) Non-contact
SLA, XJRP-SPS600, 0.1 mm layers Ra about 17 µm at 10° Falls with angle Ra about 3 µm at 90° Contact
SLA, Lite-450, UTR9000 Ra about 1.49 to 2.6 µm horizontal Not reported Ra about 6 to 30 µm vertical Contact
LPBF, Ti6Al4V Ra 9.38 ± 0.85 µm (369 µin) 5.75 ± 0.34 µm at 45° 3.18 ± 0.17 µm (125 µin) Optical, Alicona

Sources: Golhin and co-authors, Table 10 for the SLA rows; Discover Applied Sciences study on Ti6Al4V building directions for the LPBF row.

The rows do not agree with each other, and that is the lesson. On the ProJet the shallow angles are the rough ones and the vertical face is the smoothest of all. The XJRP machine shows roughness falling steadily from 10° to 90°. For the Lite-450, the vertical face is far rougher than the horizontal one. The same word, SLA, covers different machines, resins, layer thicknesses and laser settings, and the direction of the effect is a property of the setup.

A study on a desktop SLA printer in the same review table found that build orientation changed roughness while the model being solid or hollow did not, and that the staircase on bent or sloped surfaces came from the supports and the orientation together. The multi-process study found that on its masked SLA samples at 0.05 mm (0.002 in) layers the staircase was present but less marked than on material extrusion parts at 0.08 mm layers, and that the vertical faces read slightly higher.

The Shallow-Angle Trap

The multi-process study found its maximum areal roughness on extruded parts at intermediate angles, 15° to 30°, where only a few layers form the face. Its authors note that this differs from the common assumption that 45° is the worst angle. A face tilted only a little from horizontal is built from few, wide steps, and each step edge is exposed.

Top, Bottom and Side Faces in a Powder Bed

Powder bed parts are built inside a cake of hot powder, and their skin forms where fused material meets loose grains. That changes how orientation acts.

The multi-process study found no statistically significant dependence of SLS roughness on the print angle, and called its SLS topography the most isotropic of the four processes, dominated by deep pores and fused grain aggregates. A study of 50 PA12 parts on a 3D Systems ProX SLS 6100, in five orientations and three zones of the chamber, found the opposite emphasis for some faces: roughness was governed mainly by orientation, most strongly on the bottom face, while the side faces stayed largely unaffected. Position in the chamber had no significant effect on roughness in that study, though it did move positional accuracy by up to 0.1 mm (0.004 in) toward the edges of the platform.

The two results fit together once faces are separated. Side walls in a powder bed are similar whatever the part’s angle. Down-facing and up-facing surfaces are where orientation shows, and the ProX study found horizontal orientations gave better roughness than vertical ones.

MJF Faces and the Detailing Agent

One study in the review compared SLS on an EOS Formiga P110 with MJF on an HP 4200. Top faces of both measured close to 15 µm Ra, but the bottom faces split: 14.40 µm for SLS and 6.31 µm for MJF. The authors attribute the smoother MJF bottom to the detailing agent the process jets at part edges. Another study in the same table found that both SLS and MJF parts varied by their position on the platform because of thermal bleeding, and that the cube nearest the platform center had a skewed, spiked height distribution.

Layer Height and Powder Condition

A study of PA12 on a Sinterit Lisa found that laser power and chamber temperature did not significantly affect roughness, while layer height and orientation did. Rz ranged from 34.9 to 43.5 µm (1,374 to 1,713 µin) across its runs, with the highest values at its thickest layer of 0.175 mm (0.0069 in), and its lowest roughness came with thinner layers and the part parallel to the build plane. The same paper notes that fresh powder tends to give smoother surfaces than recycled or aged powder.

In a powder bed the side walls look alike at any angle. The faces that change with orientation are the ones facing down onto the cake and up out of it.

Upskin and Downskin Roughness on Metal Overhangs

Metal LPBF behaves more like a powder bed polymer on its walls and more like a staircase on its overhangs. The down-facing side of an overhang, the downskin, is melted over loose powder and picks up partly fused particles; the up-facing side, the upskin, shows the steps.

Colibrium Additive publishes a platform stability build for 316L on its M2 Series 5 at 400 W and 50 µm (0.002 in) layers: 16 positions across the plate, 64 roughness measurements per surface type. Sidewalls, 60° upskins and 60° downskins all measured a mean Ra of 8 µm (315 µin) with a standard deviation of 1 µm, and the sheet notes that the values depend on part and layout and may differ from its typical values. Its surface parameter set at 25 µm layers is offered for the best surface quality on overhang downskins and upskins.

The Ti6Al4V study in Table 2 shows how strong the angle effect can be on a metal: Ra fell from 9.38 µm at 0° to 3.18 µm at 90°, an inverse relation between roughness and building direction. At 0° and 45° the authors saw unmelted powder particles on the surface; at 90° those particles were gone and a wave-like melted surface remained.

Gränges states on its AlSi10Mg sheet that surface quality depends on orientation and on parameters such as layer thickness, and that its values indicate what can be expected. AddUp notes that its values depend on orientation and testing method and averages front, side and back surfaces.

Measuring Roughness on Printed Surfaces

Two parts with the same surface can report different roughness if they were measured differently. The review is direct about this: assessing the roughness of printed polymer surfaces requires identifying the evaluation method first.

Table 3. Roughness parameters, standards and measuring settings named in the sources
Item What it is Named in
Ra, Rz, profile parameters Average and peak-to-valley height along a traced line ISO 21920-2, with ISO 4287 still widely used, per the review
Sa, Sz, areal parameters The same quantities over an area ISO 25178-2, per the review
Rk family Parameters for plateau and valley surfaces DIN ISO 13565-1 and -2, Gränges sheet
Cutoff λc 2.5 mm (0.098 in) Filter length separating roughness from waviness ProX SLS study, Gaussian filter, N = 5; AddUp sheet
Contact stylus Profile traced by a probe Lisa, ProX and several review studies
Optical focus variation Areal topography from a microscope Ti6Al4V study; multi-process study on replicas

Sources: Golhin and co-authors, section on roughness measurement and Tables 3 and 4; the studies and datasheets named in each row.

The review lists the traps. Optical methods suit smooth polymer faces but are sensitive to reflection and translucence; fringe projection and confocal microscopy read higher and are prone to outliers; tactile probes can mark soft polymers. One cited comparison found computed tomography roughness diverged substantially from confocal microscopy on the same parts, and that shorter measuring lengths gave higher average roughness. The multi-process study measured on silicone replicas because white nylon, light resins and clear acrylics scattered or passed the microscope’s light.

For a buyer, the consequence is short. A roughness value without its parameter, instrument, cutoff and measured face is a number that cannot be checked at incoming inspection.

Bead Blasting and Finishing Before Measurement

Most printed parts are cleaned or blasted before they ship, so the as-printed values above are rarely the surface a buyer receives. The sources give a few measured effects.

  • On AlSi10Mg, AddUp reports vertical Ra falling from 6 to 8 µm as built to 4 to 7 µm after blasting with glass medium at 2 bar (29 psi).
  • On Ti6Al4V, sandblasting with alumina reduced Ra by 68.3 % at 0°, 44.1 % at 45° and 52.7 % at 90°; acid etching alone lowered roughness slightly at 0° and raised it slightly at 45° and 90°.
  • On SLA, one study in the review found roughness remarkably reduced after a wax emulsion coating.
  • On Colibrium 316L, a dedicated surface parameter set at thinner layers is the maker’s own lever before any finishing.

The order of operations matters for inspection. A drawing that states roughness should also state whether it applies as printed or after the finish, and on which faces. The same figures decide how much sanding a print needs when it serves as the master for a silicone mold that copies the printed surface as it is.

Writing a Roughness Requirement for a Printed Part

The data above lead to a few lines that make a roughness requirement mean the same thing to the buyer, the supplier and the inspector.

  1. State the parameter and its standard: Ra to ISO 21920-2 or Sa to ISO 25178-2, never just “roughness”.
  2. Name the face and its orientation in the build: top, bottom, side, upskin or downskin. Mark build direction on the drawing.
  3. Give the cutoff or measuring area and the instrument type.
  4. Say whether the value applies as printed or after blasting, smoothing or machining.
  5. For sealing or sliding faces, choose the orientation for that face first and accept the cost in time or supports, as the multi-process study recommends for critical surfaces.
  6. Ask for measured values on first parts in the actual orientation, since published values belong to their own machines and settings.

A process choice made for roughness alone settles most of the question before orientation enters: resin for a smooth as-printed skin, a powder bed for a textured one that orientation moves only on the faces facing up or down. For a buyer weighing low-volume 3D printing against a molded part for bridge production, the roughness line on the drawing is where that choice gets written down.

Sources and Further Reading

Send the 3D File of Your Printed Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with 3D Printing chosen.

Request a Quote