Surface roughness is the fine texture of a part’s surface, stated as Ra, Rz or Sa and measured by stylus or another method. On printed metal it depends on the build angle, the laser settings and the finishing steps. EOS notes that its values depend on the measurement method. A roughness value is written with its measure and the surfaces it applies to.

As-Built 316L

The May 2014 EOS sheet gives vertical 316L faces as Ra 13 ± 5 µm (512 ± 197 µin). It gives Rz as 80 ± 20 µm (3,150 ± 787 µin). Shot peening brings Ra to 5 ± 2 µm (197 ± 79 µin), and polishing brings Rz below 1 µm (39 µin). Sloping and curved faces show a stair-step effect.
Read More

Build Angle

The later EOS sheets chart Sa against the build angle of the specimen, from 45 to 90 degrees, for upward and downward faces. The chart values are not printed as numbers. A buyer therefore asks the supplier for the figure on the actual surface. Roughness by build angle is one of the part results the 316L sheet reports, the third layer of testing in ISO/ASTM 52927.

Laser Settings

In a 316L thin-wall study, vertical wall roughness rose with laser power, from Ra 13.94 to 21.35 µm (549 to 841 µin). On 10 mm (0.39 in) cubes it rose from 13.61 to 23.99 µm (536 to 944 µin). At higher power the top of a thin wall carried humps of about 200 µm (0.008 in).

Roughness Callout

An order marks each surface and gives its roughness with the measure, Ra, Rz or Sa, and the stage at which it is measured. Stylus measurement is the method MakerVerse lists for roughness. A roughness of Ra 13 µm sits inside any size measured on that face.

Orienting and Supporting a Part for SLA Printing

SLA orientation is set for the critical and cosmetic faces first, then checked for overhangs, cross section, trapped resin and support marks before anything is printed.

The Orientation Step in OrderThe order below follows Carbon's published assessment criteria for orientation and supports, with Stratasys's design guide filling in thresholds.

Surface Roughness of 3D Printed Parts by Process and Orientation

Process sets the floor of roughness and orientation moves it face by face, so a printed part's roughness note names the parameter, the face, its build direction and the finish.

Typical Ra and Sa of SLA, SLS, MJF and Metal SurfacesA review of as-printed polymer roughness in the International Journal of Advanced Manufacturing Technology collects dozens of studies by process. Another study printed one test artifact on four processes and measured them all the same way.

TPU Flexible Powder for SLS and MJF Parts

TPU from a powder bed is equally soft in every direction but stretches far less across its layers, so grade, machine, build direction and test method all belong in the order.

TPU Powder Grades and Their Tensile Properties in XY and ZFour makers' sheets give enough to compare. Forward AM, the additive business of BASF, publishes four Ultrasint TPU powders side by side in one brochure, which makes it the cleanest set: the same company, the same tests, four grades.

AlSi10Mg Aluminum Properties in Laser Powder Bed Fusion

Printed AlSi10Mg is stronger than the cast alloy as built, and the heat treatment named on the order decides how much strength is traded for ductility or conductivity.

AlSi10Mg Tensile and Yield Strength by Heat TreatmentThe first answer a buyer needs is the strength in each state the material is delivered in. Two makers publish it for their own systems and parameters, and their numbers are close enough to read together and different enough to show why the state and the source both travel with a figure.

Metal 3D Printing Stress Relief and Build Plate Removal Step by Step

Stress relieve metal parts on the plate, then cut, remove supports, anneal if needed and measure after the heat.

Metal Powder Bed Fusion Post-Build Steps in OrderThe post-build sequence for a part built on a plate has a stable shape across machine makers, because the stresses behave the same way. The sources agree on the order; they differ in how much of the detail they publish.

316L Thin Wall and Gap Dimensional Error in Laser Powder Bed Fusion

Printed metal walls and gaps land off the drawing by an amount the laser settings control, so a requirement names the parameter set, the gap needed and the finished size.

Thin Wall and Gap Error in 316L Laser Powder Bed FusionThe machine maker states accuracy as a band. EOS's sheet for 316L, dated May 2014, gives a typical achievable part accuracy of about ±20 to 50 µm (±0.0008 to 0.002 in) for small parts and about 0.2 % for large parts, and a minimum wall thickness of about 0.3 to 0.4 mm (0.012 to 0.016 in).

ISO/ASTM 52927 Main Characteristics and Test Methods for AM Parts

The test methods standard links the characteristics of additive feedstock and parts to test procedures, and a buyer fixes the method, specimen, orientation and statistical basis in the order.

What ISO/ASTM 52927 Covers and Who It Is ForThe scope states that the document specifies the principal requirements applied to the testing of parts produced by additive manufacturing processes. It does three things.

Send the 3D File of Your Printed Part

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with 3D Printing chosen.

Request a Quote