A printed 316L tensile bar pulled across the layers reaches 49 % elongation on EOS’s own sheet, while a bar pulled along the layers breaks at 38 %. That is the opposite of what a polymer powder bed does, and it surprises buyers who expect the build direction to cost ductility in every printed material. In 316L the direction costs strength instead: the vertical bar yields at 480 MPa (69.6 ksi) against 540 MPa (78.3 ksi) for the horizontal bar, both measured on the same 20 µm parameter set with several hundred specimens behind each figure.
Laser powder bed fusion (L-PBF, sold by EOS as DMLS) melts a thin layer of metal powder with a fiber laser, layer after layer, inside an argon or nitrogen atmosphere. This piece reads the published EOS data for 316L stainless steel, the grade most often asked for in stainless printed parts. It covers what the chemistry is, what the strength and ductility look like by direction, what changes between layer thicknesses, and what heat treatment and surface finish do to a part before it reaches a drawing tolerance.
What 316L Is in a Laser Powder Bed Machine
316L is a molybdenum-alloyed austenitic stainless steel. EOS markets its powder as a marine-grade steel with enhanced corrosion resistance in chloride environments, and it lists high ductility, high strength and high corrosion resistance as the main characteristics. Typical applications on the sheet include the chemical industry, food processing and medical devices, though the sheet itself gives no declaration for any of them and a buyer has to read that wording as a list of uses the powder maker has in mind.
The “L” means low carbon. The EOS powder specification caps carbon at 0.03 weight percent, which sits alongside the chromium carbide caution in the heat treatment section below.
What the machine contributes is the structure. Each layer of powder is 20 to 80 µm thick depending on the parameter set, a 400 W Yb fiber laser on the EOS M 290 scans at up to 7.0 m/s with a 100 µm focus diameter, and the part grows inside a build volume of 250 × 250 × 325 mm (9.85 × 9.85 × 12.8 in). Every property below belongs to that combination of powder, machine and parameter set, and EOS states plainly that its tolerance intervals “are not directly transferable to other systems.”
A 316L figure belongs to a machine, a layer thickness and a build direction. Read the sheet for the parameter set the supplier actually runs.
316L Powder Chemistry and Particle Size
Table 1 gives the powder composition from the EOS sheet. The sheet notes that the chemical composition corresponds to ASTM F138, the standard specification for wrought 18Cr-14Ni-2.5Mo stainless steel for surgical implants (UNS S31673), and that built parts are compliant with the powder composition.
| Element | Minimum | Maximum |
|---|---|---|
| Iron (Fe) | balance | balance |
| Chromium (Cr) | 17.00 | 19.00 |
| Nickel (Ni) | 13.00 | 15.00 |
| Molybdenum (Mo) | 2.25 | 3.00 |
| Carbon (C) | none stated | 0.03 |
| Nitrogen (N) | none stated | 0.10 |
Source: EOS material data sheet for StainlessSteel 316L. The generic particle size distribution is 20 to 65 µm, and the process data call for a 63 µm sieve.
A sheet that says the composition “corresponds to” ASTM F138 is a statement about chemistry. It does not make the printed part an implant, and it does not stand in for the manufacturer’s conformity process for a medical device. The ratings and declarations for such use sit with the maker of the finished part.
Why the Powder Size Matters to the Part
The powder fraction is bounded by the layer thickness. A 20 to 65 µm distribution sits under a 63 µm sieve, so the coarsest particles that reach the bed are about as thick as a 40 to 80 µm layer and three times a 20 µm layer. The sheet does not say how the distribution is matched to each layer thickness, so the sieve and the distribution are facts a buyer can ask about and the matching is not.
As-Built Strength and Ductility by Build Direction
EOS publishes a table per machine and layer thickness, each from its own validation data. Table 2 collects four of them, tested to ISO 6892-1 in the as-manufactured state.
| Parameter set | Direction | Yield Rp0.2 | Tensile Rm | Elongation A | Specimens |
|---|---|---|---|---|---|
| M 290, 20 µm (TRL 9) | vertical | 480 MPa (69.6 ksi) | 560 MPa (81.2 ksi) | 49 % | 363 |
| M 290, 20 µm (TRL 9) | horizontal | 540 MPa (78.3 ksi) | 645 MPa (93.6 ksi) | 38 % | 246 |
| M 290, 40 µm (TRL 7) | vertical | 490 MPa (71.1 ksi) | 580 MPa (84.1 ksi) | 49 % | 162 |
| M 290, 40 µm (TRL 7) | horizontal | 530 MPa (76.9 ksi) | 630 MPa (91.4 ksi) | 41 % | 72 |
| M 400-4, 40 µm (TRL 7) | vertical | 490 MPa (71.1 ksi) | 590 MPa (85.6 ksi) | 45 % | 120 |
| M 400-4, 40 µm (TRL 7) | horizontal | 550 MPa (79.8 ksi) | 650 MPa (94.3 ksi) | 40 % | 96 |
| M 290, 40 and 80 µm (Core, TRL 3) | vertical, both | 450 MPa (65.3 ksi) | 550 MPa (79.8 ksi) | 50 % at 40 µm, 45 % at 80 µm | not stated |
| M 290, 40 and 80 µm (Core, TRL 3) | horizontal, both | 500 MPa (72.5 ksi) | 600 MPa (87.0 ksi) | 35 % | not stated |
Source: EOS 316L material data sheet, ISO 6892-1. The Core row is described on the sheet as typical properties.
Read down the yield column and the pattern repeats on every machine: the vertical bar is 40 to 60 MPa weaker than the horizontal bar. On the first line the gap is 60 MPa, 11 % of the horizontal yield, and the tensile strength gap is 85 MPa, 13 % of the horizontal figure. In return the vertical bar stretches 29 % further than the horizontal bar on that set (49 against 38), since 49 divided by 38 is 1.29.
EOS prints a tolerance interval beside each result. For the 20 µm set the interval is a T99, the lower bound where 99 % of the population falls with 95 % confidence, and the lower bounds on the chart run from 413 to 605 MPa across the four strength figures and sit at 32 to 33 % for elongation. For the M 400-4 set the interval is a T90 and for the 40 µm set a T95. Those are three different confidence levels, so a buyer cannot lay one set’s lower bound over another’s without noting the level.
TRL is the technology readiness level EOS assigns to each parameter set. The 20 µm Surface set is stated to be validated to TRL 9, the 40 µm sets to TRL 7, and the Core set is at TRL 3. A drawing that names a TRL 3 parameter set is asking for the least validated of the four.
Printed 316L is weaker across the layers and more ductile across them. The reverse of a polymer powder bed, and the reason to state the load direction beside every strength figure.
Layer Thickness Choices and What They Change
The sheet separates its parameter sets by layer thickness and machine, and most of the practical differences sit in the process information and not in the mechanical table. Table 3 compares what is published.
| Item | M 290, 20 µm | M 290, 40 µm | M 400-4, 40 µm | M 290, 40 and 80 µm Core |
|---|---|---|---|---|
| Minimum wall thickness | 0.3 to 0.4 mm (0.012 to 0.016 in) | 0.1 mm (0.004 in) | not stated | not stated |
| Typical dimensional change after heat treatment | +0.02 % | +0.2 % | not stated | not stated |
| Volume rate | 2.0 mm³/s | 3.7 mm³/s | 14.8 mm³/s | 3.7 and 8.4 mm³/s |
| Average defect percentage | 0.018 % (45 samples) | 0.015 % (20 samples) | 0.015 % (40 samples) | 0.1 % at 40 µm, below 0.2 % at 80 µm |
| Average density (ISO 3369) | at least 7.97 g/cm³ | at least 7.97 g/cm³ | at least 7.9 g/cm³ | not stated |
Source: EOS 316L material data sheet. The 40 µm M 290 set uses the EOS grid nozzle; the 20 µm set uses the standard nozzle. Both run argon with a 63 µm sieve.
Four points follow from the table.
- Build rate and detail trade against each other, as expected. The 80 µm set in the Core family reaches 8.4 mm³/s, which EOS calls more than double the 40 µm set and states as a 100 % productivity increase over the 40 µm FlexLine set.
- The density figure of at least 7.97 g/cm³ (0.288 lb/in³) and a defect share near 0.02 % describe a part that is nearly fully dense under the ISO 3369 test. The Core set shows an average defect percentage several times higher, and EOS adds that the defect share varies with platform position.
- The dimensional change after heat treatment differs by a factor of ten between the 20 µm and the 40 µm sets. On a 100 mm dimension that is +0.02 mm against +0.2 mm, and the second figure is larger than a small-part tolerance of ±0.05 mm.
- The minimum wall of 0.1 mm on the 40 µm set is a smaller number than the 0.3 to 0.4 mm of the 20 µm set, which a reader would not predict from layer thickness alone. The sheet gives no reason, and a buyer should ask which set a given wall was designed for before relying on either number.
Typical Part Accuracy From the Older Sheet
An earlier EOS sheet for 316L, dated May 2014 for the EOSINT M280 and the M 290 on the first parameter set, states a typical achievable part accuracy of about ±20 to 50 µm (±0.0008 to 0.002 in) for small parts and about 0.2 % for large parts. A footnote says the basis is users’ experience of typical geometries, with about 40 µm when parameters can be tuned for a class of parts and about 60 µm when a new kind of geometry is built for the first time. EOS adds that accuracy depends on data preparation and post-processing.
A worked case with assumed sizes: a 200 mm part held to 0.2 % varies by ±0.4 mm. A 20 mm feature held to the small-part figure varies by ±0.02 to 0.05 mm. The two bands differ by a factor of eight to twenty, which is why one tolerance for the whole drawing is a request the process cannot meet.
Stress Relief, Solution Annealing and the Carbide Window
EOS gives two heat treatments for 316L. A stress relief holds at 900 °C (1,652 °F) for at least 2 hours once the part is thoroughly heated, then quenches in water or high-speed gas. A solution anneal holds at 1,150 °C (2,102 °F) for at least 1.5 hours, with the same quench. For both, EOS states that the cooling rate has to be high enough to prevent chromium carbide precipitation.
The older sheet adds two cautions. Parts are not ideal in the 427 to 816 °C (801 to 1,501 °F) range, because chromium carbides precipitate there, and solution annealing is not required to meet the as-built properties against ASTM A403. It also says parts show some anisotropy from the layer-wise build, which the tensile table above quantifies. Parts can be machined, shot-peened and polished as built or after stress relief to AMS 2759.
Thermal expansion matters for any part that runs hot or is heat-treated after machining. EOS data under ASTM E228 give the mean coefficient of 15.72 × 10⁻⁶ per K from 25 to 100 °C, 16.75 × 10⁻⁶ from 25 to 200 °C, 17.27 × 10⁻⁶ from 25 to 300 °C and 17.70 × 10⁻⁶ from 25 to 400 °C. A 100 mm dimension heated from 25 to 200 °C grows by 16.75 × 10⁻⁶ × 175 K × 100 mm, which is about 0.29 mm (0.012 in).
Heat Treatment and the Dimension on the Drawing
The data link back to Table 3. A part heat-treated after printing changes size by the amount in the “typical dimensional change” row, and the sheet states it for the parameter set, not for the geometry. A drawing that sets a tight dimension should say whether it applies before or after heat treatment, and who compensates for the change.
Surface Roughness and Machining Allowance
As built, the surface of a 316L part is rough, and the roughness depends on the angle of the surface to the build plate. The 2014 sheet quotes, for vertical surfaces, Ra 13 ± 5 µm (0.5 ± 0.2 × 10⁻³ in) and Rz 80 ± 20 µm as manufactured, Ra 5 ± 2 µm after shot peening and Rz below 1 µm after polishing. It adds that sloping and curved surfaces show a stair-step effect and that values depend on the measurement method.
The later sheets chart roughness against the build angle of the specimen from 45 to 90 degrees, for the upward-facing skin and the downward-facing skin, and quote Sa for the 40 µm sets. The chart values are not printed as numbers in the text of the sheet, so a buyer reads from the chart and asks the supplier for the figure on the actual surface.
The practical rule for a sealing face, a bearing seat or a thread is to treat the printed surface as a stock allowance. A supplier has to add material to the feature, then machine it, and the drawing has to say so. A surface that needs Rz below 1 µm needs polishing. Faces that carry a seal, a bearing or a thread are therefore left with stock and finished afterwards, so a printed 316L part often reaches its drawing as a printed blank with machined steel faces.
Printed 316L is a near-net-shape blank for any surface that seals, slides or threads. The finish and the final dimension belong to a second operation.
Writing a 316L Requirement a Supplier Can Quote
The following lines turn the data above into a purchase specification.
- Name the powder and the parameter set: EOS StainlessSteel 316L, machine, layer thickness and parameter set name.
- State the load direction of the critical features against the build direction, because yield differs by 40 to 60 MPa between vertical and horizontal.
- State the condition: as built, stress relieved at 900 °C, or solution annealed at 1,150 °C, and whether dimensions apply before or after.
- Mark which surfaces are as built, shot-peened, machined or polished, with the roughness value and its measure (Ra, Rz or Sa).
- Ask for density by ISO 3369 and tensile properties by ISO 6892-1 on witness specimens from the same build.
- Ask for any medical, food contact or corrosion claim as a written declaration from the part’s maker.
For a part count between one prototype and several thousand, a buyer comparing low-volume 3D printing in metal with machined stock or a cast tool in bridge production can use the same lines as a purchasing checklist for every lot.
Sources and Further Reading
- EOS GmbH, Material Data Sheet EOS StainlessSteel 316L with process data for EOS M 290 (20 µm and 40 µm), EOS M 400-4 (40 µm) and the Core 40/80 µm sets. https://www.eos.info/metal-solutions/metal-materials/data-sheets/mds-eos-stainlesssteel-316l-4441
- EOS GmbH, Process data sheet EOS StainlessSteel 316L for EOS M 290, 40 µm. https://www.eos.info/metal-solutions/data-sheets/stainlesssteel/pds-eos-stainlesssteel-316l-4404-eos-m-290-40um
- EOS GmbH, Material data sheet EOS StainlessSteel 316L, HHE/05.2014 (typical part accuracy, roughness, heat treatment cautions). https://www.eos.info
- EOS GmbH, EOS M 290 brochure, status 04/2014 (build volume, laser, scan speed, atmosphere). https://www.eos.info